Beneficiation method for zinc oxide mine

A technology of zinc oxide ore and beneficiation method, applied in chemical instruments and methods, flotation, wet separation, etc., can solve the problems of long flotation time, low recovery rate, high consumption of flotation reagents, and reduce consumption. , Improve the recovery rate and reduce the effect of zinc oxide content in tailings

Inactive Publication Date: 2006-08-23
陈铁 +1
View PDF0 Cites 54 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0003] In order to overcome the disadvantages of low recovery rate, high flotation agent consumption, long flotation time and high cost in the prior art, the present invention provides a high recovery rate and low chemical agent consumption according to the floating characteristics of argillaceous zinc oxide ore. Mineral processing method of argillaceous zinc oxide ore with small amount and high working efficiency

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Beneficiation method for zinc oxide mine
  • Beneficiation method for zinc oxide mine
  • Beneficiation method for zinc oxide mine

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0050] Raw materials: Jinding Fenghuangshan Zinc Oxide Mine in Lanping, Yunnan Province, the grade of raw ore zinc is 6.20%.

[0051] The above raw ore is subjected to the following process steps:

[0052] A. Grinding the above-mentioned argillaceous zinc oxide ore, so that the particle size is -0.1mm and accounts for 60%;

[0053] B, classifying and overflowing the pulverized ore pulp, and flotation the lead oxide ore therein with existing technology;

[0054] C. Send the tailings of lead flotation into the mixing tank, control the pulp concentration at 25%, add the following flotation agents: gangue inhibitor: water glass 500g / t, calcium lignosulfonate 150g / t; activator : Sodium sulfide 4kg / t; compound stearyl amine main collector: 180g / t stearyl amine, 50g / t acetic acid, 100g / t kerosene, 100g / t terpineol oil, 30g / t butyl ammonium black medicine; Emulsified auxiliary collector: butyl ammonium black drug 80g / t, kerosene 60g / t, Pingpingjia 40g / t, and control the pH value of ...

Embodiment 2

[0061] Raw material: the raw material belonging to the same mine as in Example 1, and its raw ore zinc grade is 9.13%.

[0062] The above-mentioned raw materials are subjected to the following process steps:

[0063] A. Grinding the above-mentioned argillaceous zinc oxide ore, so that the particle size is -0.1mm and accounts for 50%;

[0064] B, classifying and overflowing the pulverized ore pulp, and flotation the lead oxide ore therein with existing technology;

[0065] C. Put the tailings of lead flotation into the mixing tank, control the pulp concentration at 30%, add the following flotation agents: gangue inhibitor: water glass 900g / t, sodium humate 350g / t; activator: Sodium sulfide 6kg / t; compound stearyl ammonium main collector: stearyl ammonium 200g / t, acetic acid 50g / t, kerosene 150g / t, terpineol oil 200g / t, butylammonium black medicine 40g / t; Turbid liquid collector: butyl xanthate 100g / t, butyl ammonium black medicine 80g / t, gasoline 70g / t, Tween 60g / t, control t...

Embodiment 3

[0072] Raw material: Zinc oxide ore with high silicon content, the raw ore zinc grade is 8.05%.

[0073] The above-mentioned raw materials are subjected to the following process steps:

[0074] A. Grinding the above-mentioned argillaceous zinc oxide ore, so that the particle size is -0.1mm and accounts for 70%;

[0075] B, classifying and overflowing the pulverized ore pulp, and flotation the lead oxide ore therein with existing technology;

[0076] C. Send the tailings from lead flotation into the mixing tank, control the pulp concentration at 30%, add the following flotation agents: gangue inhibitor: water glass 2000g / t, ferrous sulfate 300g / t, sodium humate 200g / t; activator: sodium sulfide 5kg / t; composite octadecylamine main collector: stearylamine 240g / t, acetic acid 60g / t, kerosene 180g / t, terpineol oil 150g / t, butyl ammonium Black powder 50g / t; emulsion collector: butyl xanthate 100g / t, butyl ammonium black powder 70g / t, gasoline 70g / t, Tween 60g / t, control the pH va...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The beneficiation method for zinc oxide ore includes milling, lead oxide floating, 1-3 grade of fine grain roughing of the tailings after lead oxide floating, 1-3 times of beneficiation for each roughed concentrate, roughing the middlings of the last time and the middlings of the first beneficiation, and final precise floating to obtain the concentrate. The present invention solves the technological problem of floating muddy zinc oxide ore by means of first floating of small grains and then the large grains, and has high zinc oxide ore recovering rate, reduced zinc oxide content in the tailings, lowered floating agent consumption and effective utilization of muddy zinc oxide ore.A

Description

technical field [0001] The invention relates to a beneficiation method, in particular to a beneficiation method of argillaceous zinc oxide ore. Background technique [0002] At present, for argillaceous zinc oxide ore with high iron content, the limonite and goethite in it are easy to muddy after grinding and adhere to the surface of zinc oxide. When it is flotation, it is not easy to float; The second is that the consumption of reagents is large; the third is that the flotation time is long and the recovery rate is low. The prior art methods for flotation of argillaceous zinc oxide ore include: (1) heating, sulfidation of zinc oxide ore flotation, which not only consumes a lot of heat, but also is difficult to achieve better technical and economic indicators. (2) Sorting method of ore sand and ore slime, this method needs two processes, and the equipment that is equipped with is more, and the flotation reagent of ore slime consumes a lot, and the flotation time is long. (...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): B03D1/00B03D1/018B03D1/004B03B1/00B03B7/00B03D101/06B03D101/02B03D103/04
Inventor 陈铁杨佳定
Owner 陈铁
Who we serve
  • R&D Engineer