Method for preparing single dispersion triangular nano silver slice
A nano-silver flake, monodisperse technology, applied in the field of preparation of monodisperse triangular nano-silver flakes, can solve the problems of increasing the difficulty of production operations, unfavorable large-scale production, high equipment requirements, etc., and achieves low equipment requirements, low cost, and high technology simple effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0014] Embodiment 1: average side length is 92 ± 9nm ( figure 1 The preparation method of the triangular nano-silver sheet of e), its steps are:
[0015] (1) 480 milliliters of ternary solution systems containing water (6wt%) / PVP (K30, 5wt%) / n-amyl alcohol (89wt%) are prepared in a covered reaction vessel;
[0016] (2) 24 ml AgNO 3 (0.6wt% of the ternary solution system) the ethanol solution was added to the system under stirring, and after continuing to stir for 5 minutes, put it into a constant temperature box for heat treatment at 95° C. for 48 hours;
[0017] (3) centrifuging the heat-treated reaction solution to obtain high-purity triangular silver nanosheets of required size.
Embodiment 2
[0018] Embodiment 2: average side length is 120 ± 11nm ( figure 1 The preparation method of the triangular nano-silver sheet of f), its steps are:
[0019] (1) 480 milliliters of ternary solution systems containing (6wt%) / PVP (K30, 7wt%) / n-amyl alcohol (87wt%) are prepared in a covered reaction vessel;
[0020] (2) 24 ml AgNO 3 (0.6wt%) ethanol solution was added to the system under stirring, and after continuing to stir for 5 minutes, put it into an incubator for heat treatment at 95° C. for 48 hours;
[0021] (3) centrifuging the heat-treated reaction solution to obtain high-purity triangular silver nanosheets of required size.
Embodiment 3
[0022] Embodiment 3: the preparation method of triangular nano-silver sheet, its steps are:
[0023] (1) 480 milliliters of ternary solution systems containing water (1wt%) / PVP (K30, 29wt%) / n-amyl alcohol (70wt%) are prepared in a covered reaction vessel;
[0024] (2) 24 ml AgNO 3 (0.1wt%) ethanol solution was added into the system under stirring, and after continuing to stir for 15 minutes, put it into an incubator for heat treatment at 60° C. for 30 hours;
[0025] (3) centrifuging the heat-treated reaction solution to obtain high-purity triangular silver nanosheets of required size.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com