Paper-making grade pulp bleaching plate modifying production technique

A technology for bleaching wood pulp and production process, applied in pulp bleaching, papermaking, papermaking and other directions, can solve the problems of slow dissolution of hemicellulose, severe conditions, and difficulty in reducing polymerization, reducing production costs, increasing the content of methyl fiber, The effect of reducing pollution

Inactive Publication Date: 2008-04-09
宜宾长毅浆粕有限责任公司
View PDF2 Cites 8 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Benefits of technology

This patented technology improves on traditional processes such as papermaking and making high strength fibreboard. It involves adding special chemicals called waterproof cellulosome pitch instead of chaffyrosine to improve wetting properties while maintaining good bond between different materials like glue and cobweb threads. By doing this, these products have improved performance compared to regular wooden pulps but they also require less energy than normal ones due to their lower melting point. Additionally, there's another advantage - burning them down after leaving residual ash behind when cleanliness ends up being contaminated. Finally, the resulting product has higher stability over longer periods of storage at room temperatures.

Problems solved by technology

The technical problem addressed in this patents relates to improves the efficiency and effectiveness of producing highly purified or delicate greenish type timber without causing issues like decomposition reactions and damaged filaments after extraction. Existing methods involve acid etchings followed by alkaline immersion treatment, evaporation drying, solvent exchange, centrifugal separation, heat transferring, etc., leading to inconsistencies between batch quality control data points and product properties.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0043] Embodiment 1: caustic soda method one

[0044] 1. Use 6000Kg of paper-making grade bleached wood pulp board, and sort it by a pager.

[0045] 2. Soak into a 6.0% (3-6) pulp porridge with 8% (6-11) NaOH.

[0046]3. Use the porridge pump to send it into the press to squeeze and loosen the dispersed fibers.

[0047] 4. Put the squeezed wood pulp into the digester for cooking. The process conditions are: (1) Cooking agent: NaOH, total alkali concentration of cooking liquid 110g / l (80-120), liquid ratio 1: 3.5; (2) The initial temperature of the cooking liquid is ≥40°C; (3) pre-heating for 10-15 minutes to 105±5°C; (4) idling for 25-30 minutes after the steam is stopped; (5) 3 times of small steam release and 4 times of heating Curve, the total heating time is 2 hours; (6) The holding temperature is 155±2°C (140-168).

[0048] 5. Send the above-mentioned wood pulp slurry obtained by cooking from the dumping tank to the squeeze washing material to extract the yellow liquid...

Embodiment 2

[0052] Embodiment 2: caustic soda method two

[0053] 1. Use 6000Kg of paper-making grade bleached wood pulp board, and sort it by a pager.

[0054] 2. Soak it into a 5.0% (3-6) pulp porridge with 11% (6-11) NaOH.

[0055] 3. Use the porridge pump to send it into the press to squeeze and loosen the dispersed fibers.

[0056] 4. Put the squeezed wood pulp into the digester for cooking. The process conditions are: (1) Cooking agent: NaOH, total alkali concentration of cooking liquid 100g / l (80-120), liquid ratio 1: 3.5; (2) The initial temperature of the cooking liquid is ≥40°C; (3) pre-heating for 10-15 minutes to 105±5°C; (4) idling for 25-30 minutes after the steam is stopped; (5) 3 times of small steam release and 4 times of heating Curve, the total heating time is 2 hours; (6) The holding temperature is 168±2°C (140-168).

[0057] 5. Send the above-mentioned wood pulp slurry obtained by cooking from the dumping tank to the squeeze washing material to extract the yellow l...

Embodiment 3

[0061] Embodiment 3: caustic soda method three

[0062] 1. Use 6000Kg of paper-making grade bleached wood pulp board, and sort it by a pager.

[0063] 2. Dipping into a slurry porridge with a concentration of 4.0% (3-6) with 14% NaOH.

[0064] 3. Use the porridge pump to send it into the press to squeeze and loosen the dispersed fibers.

[0065] 4. Put the squeezed wood pulp into the digester for cooking. The process conditions are: (1) Cooking agent: NaOH, total alkali concentration of cooking liquid 80g / l (80-120), liquid ratio 1: 3.5; (2) The initial temperature of the cooking liquid is ≥40°C; (3) pre-heating for 10-15 minutes to 105±5°C; (4) idling for 25-30 minutes after the steam is stopped; (5) 3 times of small steam release and 4 times of heating curve, the total heating time is 2 hours; (6) The holding temperature is 172°C.

[0066] 5. Send the above-mentioned wood pulp slurry obtained by cooking from the dumping tank to the squeeze washing material to extract the ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention provides a denaturizing production technique of paper making bleaching wood pulp plate, which solves the problems of uneven dipping, slow hemicelluloses stripping, difficult accumulation descending, uneven cooking, single cooking method, single bleaching method and violent conditions existing in denaturizing production technique of wood pulp in the prior art. The invention comprises the following steps: wood pulp plate paging, alkali soaking, pressing, untwining and dispersion, cooking, washing, impurity removal, bleaching, a secondary washing and pulping; wherein, the wood pulp plate paging, alkali soaking, pressing, untwining and dispersion are to send papers into a alkali dipping barrel with concentration of 8 percent to 18 percent after the paper making bleaching wood pulp plates are separated by a paging device. When the wood pulp plates are changed into pulp with concentration of 3 percent to 7 percent, the pulp with concentration of 3 percent to 7 percent is sent to a squeezer to be squeezed and untwine and disperse fiber. By adopting the invention, the quality of the dissolved viscose fiber wood pulp can be better and more stable; furthermore, the invention provides wider selection range of raw material.

Description

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Owner 宜宾长毅浆粕有限责任公司
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka