Reflection watercolour for fine arts and method for manufacturing same
A technique of watercolor paint and manufacturing method, applied in the field of painting supplies
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] Embodiment one: the manufacture method of a kind of reflective watercolor pigment for fine arts of the present invention is characterized in that adopting following processing steps: its formula ratio is counted by mass parts:
[0031] First add 2 parts of gum arabic to 5 parts of distilled water, swell for 6 hours, heat to 85°C, stir until completely dissolved; then add 48 parts of water-soluble starch, 4 parts of glycerin, 0.4 parts of sodium benzoate, 2.5 parts of sodium hexametaphosphate The parts are combined and stirred evenly to make the adhesive. Add 28 parts of pigment powder titanium dioxide to the binder and stir evenly, then add 3 parts of aluminum silicate and 8 parts of hydrated silicon dioxide and stir evenly to form a coarse slurry. The coarse slurry was added to the hopper of a three-roll mill and ground for 5 times through the three-roll mill; the diameter of the three-roll mill rolls was 650 mm, and the speed of the three rolls was 26:70:145 (r.p.m). ...
Embodiment 2
[0032] Embodiment two: a kind of manufacture method of reflective watercolor pigment for fine arts of the present invention is characterized in that adopting following processing steps: its formula ratio is counted by mass parts:
[0033] First add 2.5 parts of gum arabic to 14.5 parts of distilled water, swell for 8 hours, heat to 88°C, stir until completely dissolved; add 52 parts of water-soluble starch, 4.5 parts of glycerin, 0.45 parts of sodium benzoate, and 2.0 parts of sodium hexametaphosphate After merging, stir evenly to make adhesive. Add 13 parts of pigment powder CI Pigment Red 8 to the binder and stir evenly, then add 4 parts of aluminum silicate and 7.0 parts of hydrated silicon dioxide and stir evenly to form a coarse slurry. The coarse slurry was added to the hopper of a three-roll mill and ground for 5 times through the three-roll mill; the diameter of the three-roll mill rolls was 650 mm, and the speed of the three rolls was 26:70:145 (r.p.m). Adjust the wi...
Embodiment 3
[0034] Embodiment three: a kind of manufacture method of reflective watercolor paint for fine arts of the present invention is characterized in that adopting following processing steps: its formula ratio is counted by mass parts:
[0035] First add 3.0 parts of gum arabic to 15 parts of distilled water, swell for 10 hours, heat to 90°C, stir until completely dissolved; add 50 parts of water-soluble starch, 3.5 parts of glycerin, 0.5 parts of sodium benzoate, and 3.0 parts of sodium hexametaphosphate After merging, stir evenly to make adhesive. Add 14 parts of pigment powder pigment permanent violet RL to the binder and stir evenly, then add 5.0 parts of aluminum silicate and 6.0 parts of hydrated silicon dioxide and stir evenly to form a coarse slurry. The coarse slurry was added to the hopper of a three-roll mill and ground for 5 times through the three-roll mill; the diameter of the three-roll mill rolls was 650 mm, and the speed of the three rolls was 26:70:145 (r.p.m). Ad...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com