Preparation method of aluminum alloy corrosion resistant coating

A technology of corrosion-resistant coating and aluminum alloy, which is applied in the direction of metal material coating process, coating, and the device for coating liquid on the surface, etc. Unstable corrosion resistance and other issues, to achieve high economic returns, flexible construction, and short processing time

Active Publication Date: 2011-07-27
南京南大波平电子信息有限公司
View PDF0 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, the anodic oxidation process of aluminum alloy is complicated, and it is easily affected by chemical and physical factors such as electrolyte solubility changes and current fluctuations in the chemical reaction pool, resulting in defects in the oxide layer on the surface of the aluminum alloy, resulting in unstable corrosion resistance, and the anodic oxidation process is also difficult. Does not meet current environmental protection and energy saving requirements

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Preparation method of aluminum alloy corrosion resistant coating
  • Preparation method of aluminum alloy corrosion resistant coating
  • Preparation method of aluminum alloy corrosion resistant coating

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0025] Add 18.8L of pure water (or deionized water) to a 25L stainless steel bucket, and then add 1.375Kg of ammonium nitrate (NH 4 NO 3 ), 0.65Kg cobalt nitrate (Co(NO 3 ) 2 .6H 2 O), 0.66L formic acid (HCOOH), drop 0.3mol / L ammonium hydroxide (NH 4 OH) aqueous solution to directly mix the solution pH=6.8-7.2, then add 0.325Kg sodium nitrite (NaNO 2 ), 5mL 30wt% hydrogen peroxide (H 2 o 2 ) aqueous solution, heated to 55-65° C. for 30-90 minutes under ordinary nitrogen jet stirring. Add dropwise 0.3mol / L ammonium hydroxide (NH 4 OH) aqueous solution until the reaction solution pH = 6.8-7.2, set aside.

[0026] Heat and soak the clean aluminum alloy test plate with cobalt aqueous solution at 50-65°C for 5-25 minutes, then take it out and dry it at room temperature for 24 hours, and then treat the surface of the test plate with a spray solution of oxidized polyaniline doped mercapto organic acid compound , Vacuum drying to remove excess solvent, conduct salt spray corr...

Embodiment 2

[0028] Add 16.7L of pure water (or deionized water) to a 25L stainless steel bucket, and then add 1.325Kg of ammonium nitrate (NH 4 NO 3 ), 0.65Kg cobalt nitrate (Co(NO 3 ) 2 .6H 2 O), 1L glacial acetic acid (CH 3 COOH), 20mL 30wt% hydrogen peroxide (H 2 o 2 ) aqueous solution, start a common nitrogen jet stirring device, and react for 10 to 15 minutes. Add 0.325Kg sodium nitrite (NaNO 2 ) heated to 36-42 ° C for 20-30 minutes. Then dropwise add 0.42mol / L ammonium hydroxide (NH 4 OH) aqueous solution until the reaction solution pH=6.7-7.0, finally add 5mL 30wt% hydrogen peroxide (H 2 o 2 ) aqueous solution, heated up to 55-65°C, stirred for several minutes, and set aside.

[0029] Heat and soak the clean aluminum alloy test plate with cobalt aqueous solution at 50-65°C for 5-25 minutes, then take it out and dry it at room temperature for 24 hours, and then treat the surface of the test plate with a spray solution of oxidized polyaniline doped mercapto organic acid c...

Embodiment 3

[0031] Add 18.8L of pure water (or deionized water) to a 25L stainless steel bucket under ordinary nitrogen jet stirring, and then add 1.375Kg of ammonium nitrate (NH 4 NO 3 ), 0.65Kg cobalt nitrate (Co(NO 3 ) 2 .6H 2 O), 0.66L ammonium formate (NH 4 COOH), add dropwise 0.2mol / L ammonium hydroxide (NH 4 OH) aqueous solution to directly mix the solution pH=7.0-7.1, then add 0.325Kg sodium nitrite (NaNO 2 ), 5mL 30wt% hydrogen peroxide (H 2 o 2 ) aqueous solution reaction, a slight ammonia gas is generated during the reaction, and the reaction lasts for 5-10 minutes. Then the temperature was further raised to 55-65° C. for 30-90 minutes. Add dropwise 0.2mol / L ammonium hydroxide (NH 4 OH) aqueous solution until the reaction solution pH=7.0-7.1, set aside.

[0032] Heat and soak the clean aluminum alloy test plate with cobalt aqueous solution at 50-65°C for 5-25 minutes, then take it out and dry it at room temperature for 24 hours, and then treat the surface of the test ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
thicknessaaaaaaaaaa
thicknessaaaaaaaaaa
Login to View More

Abstract

The invention relates to a preparation method of an aluminum alloy corrosion resistant coating, comprising the following steps: forming a passivation layer which has a certain nanometer thickness and contains cobalt element on the surface of aluminum alloy by adopting a chemical reaction method and further covering a sulfydryl organic acid compound doped oxidation polyaniline coating on the passivation layer. By adopting the method, the corrosion resistant characteristic of the surface of the aluminum alloy is realized through inhibiting electrochemical reaction. The invention solves the problems of complex process, unstable oxidation quality, high energy consumption, severe pollution and the like of the traditional anode oxidation, and is suitable for use in the fields of special aluminum alloy materials in the industries of navigation, spaceflight, ships and warships and the like. Compared with the prior art, the invention has the characteristics of simple method, short reaction time, little equipment investment and high economic return.

Description

technical field [0001] The invention relates to a preparation method of a high-strength, high-toughness aluminum alloy corrosion-resistant coating, in particular to the preparation of a special aluminum alloy corrosion-resistant layer for aircraft and large ships. Background technique [0002] The corrosion resistance of metal materials is a very important performance index in evaluating the service life of materials. During the operation of aircraft and ships, they must withstand severe salt, splash, spray and continuous wet / dry cycle, so that aircraft and ships are subject to extensive and serious corrosion problems. Therefore, the solution to the corrosion of aircraft and ships has received widespread attention. In recent years, with the rapid development of domestic aircraft and ship manufacturing industries, the use of high-performance aluminum alloys represented by high strength and high toughness is also increasing. Therefore, the anti-corrosion treatment of high-pe...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & AuthorityPatents(China)
IPC IPC(8): C23C22/68B05D7/16C09D179/02
Inventor胡益民汪洪陈晓东
Owner南京南大波平电子信息有限公司