Epoxy solvent free paint and preparation method thereof
A solvent-free coating and epoxy technology, applied in the field of coatings, can solve problems such as explosion, environmental and human injury, and human harm, and achieve the effects of good environmental protection, reduced number of constructions, and good acid resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] A preparation method of epoxy solvent-free coating, the method comprises the following processing steps:
[0029] (1) Add 35kg of epoxy resin, 2kg of additives, and 5kg of curing agent into the equipment, heat at 35°C and stir for 4 hours, and then the test indicators are qualified;
[0030] (2) Add 30kg of inert pigments and fillers and 3kg of additives to disperse (1200 rpm) for 45 minutes;
[0031] (3) enter the shearing machine until the detection index is qualified, and make the epoxy solvent-free coating;
[0032] (5) Send to pass the quality inspection, prepare the curing agent and pack it into the warehouse.
Embodiment 2
[0034] A preparation method of epoxy solvent-free coating, the method comprises the following processing steps:
[0035] (1) Add 40kg of epoxy resin, 5kg of additives, and 5kg of curing agent into the equipment, heat at 40°C and stir for 4 hours, and then the test indicators are qualified;
[0036] (2) Add 40kg of inert pigments and fillers and 1kg of additives to disperse (1200 rpm) for 45 minutes;
[0037] (3) enter the shearing machine until the detection index is qualified, and make the epoxy solvent-free coating;
[0038] (4) Send to pass the quality inspection, prepare the curing agent and pack it into the warehouse.
Embodiment 3
[0040] A preparation method of epoxy solvent-free coating, the method comprises the following processing steps:
[0041] (1) Add 45kg of epoxy resin, 5kg of additives, and 5kg of curing agent into the equipment, heat at 45°C and stir for 2 hours, and then the test indicators are qualified;
[0042] (2) Add 45 kg of inert pigments and fillers and 5 kg of additives to disperse (1200 rpm) for 55 minutes;
[0043] (3) enter the shearing machine until the detection index is qualified, and make the epoxy solvent-free coating;
[0044] (4) Send to pass the quality inspection, prepare the curing agent and pack it into the warehouse.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com