A processing method and fabric technology, applied in dyeing, textile and papermaking, fiber treatment, etc., can solve the problems of uneven imitation effect, high energy consumption, environmental pollution, etc., to ensure stability and production efficiency, Reduce environmental pollution and improve product quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] Embodiment one: get specification and be 20S (imperial count), the yarn that quantity is 30KG is carried out single yarn modification, and dyed into dark blue, the specific process of finally being processed into imitation old-fashioned yarn-dyed fabric is as follows:
[0025] (1) Add 80g / L modifier into the sizing tank of the single yarn sizing machine (YAMADA YS-6), let the yarn undergo cationic modification through the single yarn sizing machine, and wind the modified yarn Put the bobbin yarn on the paper tube, and then wind the bobbin on the winder (SSM TW1-W) to the plastic bobbin with holes, control the loose yarn density of the bobbin to 0.37g / cm 3 , single yarn weight is 0.5Kg / tube;
[0026] (2), put the modified bobbin in the dye vat, wash with 60°C hot water for 10min, and drain;
[0027] (3) Add water to the dye vat, add DyStar Remazol navy blue dye 2% (owf) at room temperature, stir evenly, and raise the temperature to 80°C at a rate of 2.0°C / min, keep it w...
Embodiment 2
[0029] Embodiment two: getting specification is 20S (imperial count), the yarn that quantity is 25KG is carried out single yarn modification, and dyed into navy blue, the concrete process of finally being processed into imitation old-fashioned yarn-dyed fabric is as follows:
[0030] (1) Add 60g / L modifier into the sizing tank of the single yarn sizing machine (YAMADA YS-6), let the yarn undergo cationic modification through the single yarn sizing machine, and wind the modified yarn Put the bobbin yarn on the paper tube, then wind the bobbin on the winder (SSM TW1-W) to the plastic bobbin with holes, control the loose yarn density of the bobbin to 0.32g / cm 3 , single yarn weight is 0.4Kg / tube;
[0031] (2), put the modified bobbin in the dye vat, wash with 60°C hot water for 10min, and drain;
[0032] (3) Add water to the dye vat, add DyStar Remazol navy blue dye 2% (owf) at room temperature, stir evenly, and raise the temperature to 80°C at a rate of 1.5°C / min, keep it warm ...
Embodiment 3
[0034] Embodiment three: get specification is 10S, the yarn that quantity is 50Kg is carried out skein modification, and is dyed into maroon, the concrete process of finally being processed into imitation old-fashioned yarn-dyed fabric is as follows:
[0035] (1), the yarn is shaken on the hank yarn shaking machine, the weight of the controlled yarn is 400g / turn, and the thickness of the yarn is even;
[0036] (2) Add 1g / L of refining agent into the skein jet dyeing vat, put the shaken yarn into the skein jet dyeing vat for slight refining, and heat-preserve at 95°C for 10 minutes;
[0037] (3), washing the refined yarn twice;
[0038] (4), cationic modification is carried out to yarn in hank yarn dyeing machine, wherein the consumption of adding modifier is 80g / L, and the weight bath ratio of control yarn and modifier solution is 1: 10, at 60 Insulation treatment at a temperature of ℃ for 15 minutes, and drain;
[0039] (5), the modified skein is placed in the dye vat, wash...
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com