A soil modification and slope technology, applied in soil conditioning materials, chemical instruments and methods, organic fertilizers, etc., can solve the problems of less research on slope soil modification, short-term degradation of vegetation, vegetation growth, etc., and achieve enhanced water absorption. Water retention capacity, satisfying stable growth, and improving the effect of soil and water conservation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0020] (1) Take 10 grams of polyacrylate emulsion (Wuhan Yuancheng Science and Technology Development Co., Ltd., polyacrylate emulsion), 80 grams of water, fully mix;
[0021] (2) take by weighing 3 grams of bentonite, 3 grams of kaolin, 2 grams of desulfurized gypsum, and 1 gram of fiber, fully mixing;
[0022] (3) The substance in the step (1) is gradually added to the substance in the step (2) under stirring, and the stirring time is 1 hour to form a composite emulsion;
[0023] (4) Weigh 1 gram of polyacrylamide (Gongyi Huatong Filter Material Factory, HTLPAM-2) and gradually add it to the composite emulsion in (3) under stirring, and stir until the polyacrylamide is completely dissolved in the composite emulsion , forming slope soil modification materials.
Embodiment 2
[0025] (1) Take by weighing 8 grams of polyacrylate emulsion (Wuhan Yuancheng Science and Technology Development Co., Ltd., polyacrylate emulsion), 82.5 grams of water, fully mix;
[0026] (2) take by weighing 2 grams of bentonite, 2 grams of kaolin, 2 grams of desulfurized gypsum, and 0.5 grams of fiber, fully mixed;
[0027] (3) The substance in the step (1) is gradually added to the substance in the step (2) under stirring, and the stirring time is 1 hour to form a composite emulsion;
[0028] (4) Weigh 3 grams of polyacrylamide (Gongyi Huatong Filter Material Factory, HTLPAM-2) and gradually add it to the composite emulsion in (3) under stirring, and stir until the polyacrylamide is completely dissolved in the composite emulsion , forming slope soil modification materials.
Embodiment 3
[0030] (1) Take by weighing 5 grams of polyacrylate (Wuhan Yuancheng Technology Development Co., Ltd., polyacrylate emulsion) emulsion, 84.5 grams of water, fully mix;
[0031] (2) take by weighing 2 grams of bentonite, 2 grams of kaolin, 2 grams of desulfurized gypsum, and 0.5 grams of fiber, fully mixed;
[0032] (3) The substance in the step (1) is gradually added to the substance in the step (2) under stirring, and the stirring time is 1 hour to form a composite emulsion;
[0033] (4) Weigh 4 grams of polyacrylamide (Gongyi Huatong Filter Material Factory, HTLPAM-2) and gradually add it to the composite emulsion in (3) under stirring, and stir until the polyacrylamide is completely dissolved in the composite emulsion , forming slope soil modification materials.
[0034] The composite emulsion in the above example is applied to the slope with a slope of 1:0.75 by spraying method, and the effect after one week of spraying construction is shown in Table 1.
[0035]
[00...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com