Method for locking water in wood and wood processed with same
A wood and moisture technology, applied in the field of materials, can solve the problems of mahogany furniture production, communication, use restrictions, etc., and achieve the effect of good anti-moth and anti-corrosion effect and huge economic benefits.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0042] A method of locking moisture in wood comprising the steps of:
[0043] Step 1: Under vacuum, control the gas content and moisture content of the wood that needs to lock in moisture; the moisture content is controlled at 8%, and the gas content is controlled at 0.01%;
[0044] The second step: under vacuum, put the paraffin into the container, and heat it to melt it completely; the vacuum is 0.01MPa; the straight-chain alkanes in the paraffin account for 80%; Cyclocycloalkane accounts for 2%; melting temperature is 55°C;
[0045] The third step: Put the wood obtained in the first step into the container of the second step, completely immerse the wood in the melted paraffin, keep it for 20 minutes, and keep the container in a vacuum state; the vacuum degree is 0.01MPa;
[0046] Step 4: Under vacuum, lower the temperature in the container to normal temperature, so that the molten paraffin solidifies and seals the internal gap of the wood; the vacuum degree is 0.01MPa;
...
Embodiment 2
[0050] A method of locking moisture in wood comprising the steps of:
[0051] Step 1: Under vacuum, control the gas content and moisture content of the wood that needs to lock in moisture; the moisture content is controlled at 12%, and the gas content is controlled at 0.02%;
[0052] The second step: under vacuum, put the paraffin into the container, and heat it to melt it completely; the vacuum is 0.05MPa; the straight-chain alkanes in the paraffin account for 90%; Cyclocycloalkane accounts for 3%; melting temperature is 75°C;
[0053] The third step: put the wood obtained in the first step into the container of the second step, completely immerse the wood in the melted paraffin, keep it for 50 minutes, and keep the container in a vacuum state; the vacuum degree is 0.05MPa;
[0054] Step 4: Under vacuum, reduce the temperature in the container to normal temperature, so that the molten paraffin solidifies and seals the internal gap of the wood; the vacuum degree is 0.05MPa; ...
Embodiment 3
[0059] A method of locking moisture in wood comprising the steps of:
[0060] Step 1: Under vacuum, control the gas content and moisture content of the wood that needs to lock moisture; the moisture content is controlled at 16%, and the gas content is controlled at 0.05%;
[0061] The second step: under vacuum, put the paraffin into the container, and heat it to melt completely; the vacuum is 0.1MPa; the straight chain alkanes in the paraffin account for 95%; Cyclocycloalkane accounts for 4%; melting temperature is 80°C;
[0062] The third step: put the wood obtained in the first step into the container of the second step, completely immerse the wood in the melted paraffin, keep it for 2 hours, and keep the container in a vacuum state; the vacuum degree is 0.1MPa;
[0063] Step 4: Under vacuum, reduce the temperature in the container to normal temperature, so that the molten paraffin solidifies and seals the internal gap of the wood; the vacuum degree is 0.1MPa;
[0064] Ste...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com