Embodiment 1
[0016] A polyurethane microporous elastic sports field material formula is composed of component A, component B and water, wherein the weight ratio of component A and component B is 1:3, and the total weight of water and component A and B after mixing The weight ratio is 3‰:1, component A is composed of the following components by mass percentage: polyether polyol 60%, MDI-50 40%, component B is composed of the following components by mass percentage: paraffin wax 30% , polyether polyol 20%, 400 mesh talcum powder 44, iron red 3%, white carbon black 3%.
[0017] The preparation method is as follows: (1) Weigh polyether polyol and MDI-50 according to the above formula, stir evenly, keep warm at 75°C for two hours, and then take out of the oven to obtain component A;
[0018] (2) Weigh paraffin wax, polyether polyol, talcum powder, iron red and white carbon black according to the above formula, stir them evenly in the reaction kettle and take them out of the oven to obtain compo...
Embodiment 2
[0021] A polyurethane microporous elastic sports field material formula is composed of component A, component B and water, wherein the weight ratio of component A and component B is 1:3, and the total weight of water and component A and B after mixing The weight ratio is 5‰:1, component A is composed of the following components by mass percentage: polyether polyol 80%, MDI-50 20%, component B is composed of the following components by mass percentage: paraffin wax 40% , polyether polyol 10%, talcum powder 48%, iron red 1%, white carbon black 1%.
[0022] The preparation method is as follows: (1) Weigh polyether polyol and MDI-50 according to the above formula, stir evenly, keep warm at 75°C for two hours, and then take out of the oven to obtain component A;
[0023] (2) Weigh paraffin wax, polyether polyol, talcum powder, iron red and white carbon black according to the above formula, stir them evenly in the reaction kettle and take them out of the oven to obtain component B; ...
Embodiment 3
[0026] A polyurethane microporous elastic sports field material formula is composed of component A, component B and water, wherein the weight ratio of component A and component B is 1:3, and the total weight of water and component A and B after mixing The weight ratio is 4‰:1, component A is composed of the following components by mass percentage: polyether polyol 70%, MDI-50 30%, component B is composed of the following components by mass percentage: paraffin wax 35% , polyether polyol 11%, talc 50%, iron red 2%, white carbon black 2%.
[0027] The preparation method is as follows: (1) Weigh the polyether polyol and MDI-50 according to the above formula, stir evenly, keep it at 75°C for two hours, and then take it out of the oven to obtain component A;
[0028] (2) Weigh paraffin wax, polyether polyol, talcum powder, iron red and white carbon black according to the above formula, stir them evenly in the reaction kettle and take them out of the furnace to obtain component B; ...