PU matte color repairing golden oil and preparation process thereof
A color-correcting gold oil and matte technology, applied in the field of PU matte color-correcting gold oil and its production process, can solve the problems of shortening the storage time of the coating, the influence of the stability of the coating, and the high price, so as to improve the stability performance and storage time. , Improve the leveling performance, the effect of fast drying
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] Step 1: Weigh the raw materials according to the weight ratio;
[0027] Step 2: Put styrene-modified alkyd resin and cyclohexanone into the dispersion tank, turn on the switch of the stirring device, and adjust the speed to 1000 rpm for 5 minutes;
[0028] Step 3: After the dispersion in the previous step is completed, add matting powder and increase the stirring speed to 1500 rpm for 15 minutes;
[0029] Step 4: After the dispersion in the previous step is completed, add nitrocellulose, nitropropane and absolute ethanol, and reduce the stirring speed to 1000 rpm for 10 minutes;
[0030] Step 5: After the dispersion in the previous step is completed, add polyamide wax, leveling agent, defoamer and butyl ester, reduce the rotation speed to 800 rpm, last for 5 minutes, and discharge.
Embodiment 2
[0032] Step 1: Weigh the raw materials according to the weight ratio;
[0033] Step 2: Put styrene-modified alkyd resin and cyclohexanone into the dispersion tank, turn on the switch of the stirring device, and adjust the speed to 1000 rpm for 8 minutes;
[0034] Step 3: After the dispersion in the previous step is completed, add matting powder and increase the stirring speed to 1500 rpm for 15 minutes;
[0035] Step 4: After the dispersion in the previous step is completed, add nitrocellulose, nitropropane and absolute ethanol, and reduce the stirring speed to 1000 rpm for 8 minutes;
[0036] Step 5: After the dispersion in the previous step is completed, add polyamide wax, leveling agent, defoamer and butyl ester, reduce the rotation speed to 800 rpm, last for 5 minutes, and discharge.
Embodiment 3
[0038] Step 1: Weigh the raw materials according to the weight ratio;
[0039] Step 2: Put styrene-modified alkyd resin and cyclohexanone into the dispersion tank, turn on the switch of the stirring device, and adjust the speed to 1000 rpm for 6 minutes;
[0040] Step 3: After the dispersion in the previous step is completed, add matting powder and increase the stirring speed to 1500 rpm for 15 minutes;
[0041] Step 4: After the dispersion in the previous step is completed, add nitrocellulose, nitropropane and absolute ethanol, and reduce the stirring speed to 1000 rpm for 9 minutes;
[0042] Step 5: After the dispersion in the previous step is completed, add polyamide wax, leveling agent, defoamer and butyl ester, reduce the rotation speed to 800 rpm, last for 5 minutes, and discharge.
[0043] The relevant performance test index with the present embodiment product is as follows:
[0044] Test items Example 1 Example 2 Example 3 Solid content (150℃ / 60m...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com