Novel two-component epoxy resin corrosion-resistant coating and preparation method for same
A technology of epoxy resin and anti-corrosion coating, applied in the direction of epoxy resin coating, anti-corrosion coating, coating, etc., can solve the problems of unsatisfactory anti-corrosion performance, achieve good protection effect, reduce corrosion rate, and reduce corrosion dissolution rate Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0029] A new type of two-component epoxy resin anti-corrosion coating, composed of component A and component B,
[0030] The parts by weight of component A comprise:
[0031]
[0032] The parts by weight of component B comprise:
[0033] Curing agent 15g,
[0034] Polyaniline 5g;
[0035] The mass ratio of component A and component B is 5:1.
[0036] Its preparation method comprises the following steps:
[0037] (1) Dissolve polyaniline in the curing agent and stir evenly to obtain component B;
[0038] (2) Put the components in component A together and stir evenly to obtain component A;
[0039] (3) Mix components A and B evenly at a mass ratio of 5:1 to obtain a two-component epoxy resin anticorrosion coating.
Embodiment 2
[0041] A new type of two-component epoxy resin anti-corrosion coating, composed of component A and component B,
[0042] The parts by weight of component A comprise:
[0043]
[0044] The parts by weight of component B comprise:
[0045] Curing agent 17g,
[0046] Polyaniline 3g;
[0047] The mass ratio of component A and component B is 5:1.
[0048] Its preparation method comprises the following steps:
[0049] (1) Dissolve polyaniline in the curing agent and stir evenly to obtain component B;
[0050] (2) Put the components in component A together and stir evenly to obtain component A;
[0051] (3) Mix components A and B evenly at a mass ratio of 5:1 to obtain a two-component epoxy resin anticorrosion coating.
Embodiment 3
[0053] A new type of two-component epoxy resin anti-corrosion coating, composed of component A and component B,
[0054] The parts by weight of component A comprise:
[0055]
[0056] The parts by weight of component B comprise:
[0057] Curing agent 16g,
[0058] Polyaniline 4g;
[0059] The mass ratio of component A and component B is 5:1.
[0060] Its preparation method comprises the following steps:
[0061] (1) Dissolve polyaniline in the curing agent and stir evenly to obtain component B;
[0062] (2) Put the components in component A together and stir evenly to obtain component A;
[0063] (3) Mix components A and B evenly at a mass ratio of 5:1 to obtain a two-component epoxy resin anticorrosion coating.