Photocatalyst mate
A technology of photocatalyst and companion, which is applied in the field of photocatalyst companion, can solve problems such as easy damage to furniture, health hazards, etc., and achieve the effect of convenient spraying, improved environment and fast effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] Formula: 1% citric acid monohydrate; 5% tetraethoxysilane; 0.2% penetrant JFC; 0.03% organic silicon defoamer; 0.05% phytic acid; 93.72% deionized water.
[0033] Preparation method: first add citric acid monohydrate to deionized water and stir for 10 minutes, then add tetraethoxysilane and stir for 10 minutes, then add penetrant JFC and stir for 10 minutes, then add silicone defoamer and stir for 10 minutes, and finally Add phytic acid and stir for 10 minutes. After all the ingredients are added, let it stand for 30 minutes, then pour it into the ultrafilter for ultrafiltration, and finally form the product.
Embodiment 2
[0035] Formula: citric acid monohydrate 3%; tetraethoxysilane 5%; penetrant JFC 0.1%; silicone defoamer 0.01%; phytic acid 0.01%; deionized water 91.88%.
[0036] Preparation method: first add citric acid monohydrate to deionized water and stir for 10 minutes, then add tetraethoxysilane and stir for 10 minutes, then add penetrant JFC and stir for 10 minutes, then add silicone defoamer and stir for 10 minutes, and finally Add phytic acid and stir for 10 minutes. After all the ingredients are added, let it stand for 30 minutes, then pour it into the ultrafilter for ultrafiltration, and finally form the product.
Embodiment 3
[0038] Formula: citric acid monohydrate 2%; tetraethoxysilane 7%; penetrant JFC 0.3%; silicone defoamer 0.05%; phytic acid 0.05%; deionized water 90.6%.
[0039] Preparation method: first add citric acid monohydrate to deionized water and stir for 10 minutes, then add tetraethoxysilane and stir for 10 minutes, then add penetrant JFC and stir for 10 minutes, then add silicone defoamer and stir for 10 minutes, and finally Add phytic acid and stir for 10 minutes. After all the ingredients are added, let it stand for 30 minutes, then pour it into the ultrafilter for ultrafiltration, and finally form the product.
PUM

Abstract
Description
Claims
Application Information

- Generate Ideas
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com