Embodiment 1
[0013] A preparation method of a talcum powder dispersion for papermaking, comprising the following steps:
[0014] Calcium carbonate pretreatment: Grinding, passing through a 325-mesh sieve to obtain 63% of calcium carbonate whose particle size is less than or equal to 2um.
[0015] 12g water is joined in the plastic beaker of 150ml, then add 0.6g solid content and be 40% dispersant, use low-speed stirrer to stir with 200rpm, add 60g solid content then while stirring and be 73% ground calcium carbonate, stir 2min, finally slowly add 40g of talcum powder with a solid content of 87%, stir for about 30min while adding, and finally mix to prepare the talcum powder dispersion for papermaking.
Embodiment 2
[0017] A preparation method of a talcum powder dispersion for papermaking, comprising the following steps:
[0018] Calcium carbonate pretreatment: Grinding, passing through a 325 mesh sieve to obtain calcium carbonate with a particle size of 65% less than or equal to 2um.
[0019] 9.6g water is joined in the plastics beaker of 150ml, add 0.7g solid content again and be the dispersant of 45%, use low-speed stirrer to stir with 200rpm, add 65g while stirring subsequently and be the ground calcium carbonate of 75% solid content, Stir for 2 minutes, and finally slowly add 35 g of talcum powder with a solid content of 90%, stir for about 30 minutes while adding, and finally mix to prepare a talc powder dispersion for papermaking.
Embodiment 3
[0021] A preparation method of a talcum powder dispersion for papermaking, comprising the following steps:
[0022] Calcium carbonate pretreatment: Grinding, passing through a 325 mesh sieve to obtain calcium carbonate with a particle size of 67% less than or equal to 2um.
[0023] 10.4g water is joined in the plastics beaker of 150ml, add 0.8g solid content again and be the dispersant of 50%, use low-speed stirrer to stir with 300rpm, add 70g while stirring subsequently and be the ground calcium carbonate of 77% solid content, Stir for 2 minutes, and finally slowly add 30 g of talc powder with a solid content of 90%, stir for about 30 minutes while adding, and finally mix to prepare a talc powder dispersion for papermaking.