Production process of fluorescent cloth
A production process and technology of fluorescent cloth, applied in textiles, papermaking, fiber processing, etc., can solve the problems of anti-fouling performance and washing resistance to be improved, and achieve the effect of strong washing resistance and excellent flame retardant performance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] The production process of fluorescent cloth includes the following steps:
[0025] 1) Put 5 parts by mass of dimethylolurea, 1.6 parts by mass of hexanol, and 2.3 parts by mass of phosphate into 8.3 parts by mass of deionized water and mix them evenly;
[0026] 2) At the same time, slowly add 3.7 parts by mass of tetrahydroxyethylphosphine chloride, 1.7 parts by mass of dimethylolethylene urea, and 2.8 parts by mass of sodium laurate, and continue stirring until fully mixed and uniform to prepare a finishing agent;
[0027] 3) Pad the cloth in the dipping solution containing the finishing agent, and dry it at a constant temperature.
Embodiment 2
[0029] The production process of fluorescent cloth includes the following steps:
[0030] 1) Add 6 parts by mass of dimethylolurea, 1.6 parts by mass of hexanol, and 2.3 parts by mass of phosphate ester into 8.3 parts by mass of deionized water and mix them evenly;
[0031] 2) At the same time, slowly add 3.7 parts by mass of tetrahydroxyethylphosphine chloride, 1.7 parts by mass of dimethylolethylene urea, and 2.8 parts by mass of sodium laurate, and continue stirring until fully mixed and uniform to prepare a finishing agent;
[0032] 3) Pad the cloth in the dipping solution containing the finishing agent, and dry it at a constant temperature.
Embodiment 3
[0034] The production process of fluorescent cloth includes the following steps:
[0035] 1) Add 5.6 parts by mass of dimethylolurea, 1.6 parts by mass of hexanol, and 2.3 parts by mass of phosphate ester into 8.3 parts by mass of deionized water and mix them evenly;
[0036] 2) At the same time, slowly add 3.7 parts by mass of tetrahydroxyethylphosphine chloride, 1.7 parts by mass of dimethylolethylene urea, and 2.8 parts by mass of sodium laurate, and continue stirring until fully mixed and uniform to prepare a finishing agent;
[0037] 3) Pad the cloth in the dipping solution containing the finishing agent, and dry it at a constant temperature.
PUM

Abstract
Description
Claims
Application Information

- Generate Ideas
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com