Environment-friendly concave-convex rod mineral cat litter
An attapulgite, environmentally friendly technology, applied in animal houses, applications, animal husbandry, etc., can solve problems such as harmful health, high price, dust, etc., to achieve no dust, low price, and odor absorption effect.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] An environment-friendly attapulgite mineral cat litter, comprising the steps of:
[0037] A. Broken
[0038] Break the attapulgite ore;
[0039] B. Raw material preparation
[0040] Attapulgite ore, bentonite ore and additive corn cob powder are prepared by weight, 60 parts of attapulgite ore, 15 parts of bentonite ore, and 15 parts of corn cob powder;
[0041] C. Drying and sieving
[0042] Send the raw materials into a mill and extrude them into granules with a particle size of 2-3mm. Dry them in the air to reduce the moisture content of the attapulgite clay to 15%, then crush them and sieve them to obtain attapulgites. Powder, sieve size is 100-150 mesh;
[0043] D. Baking
[0044] The sieved attapulgite powder is sent into a roasting furnace for roasting, the roasting temperature is controlled at 300° C., and the roasting time is 45 minutes to obtain the finished product environment-friendly attapulgite mineral cat litter. In the step D, the moisture content i...
Embodiment 2
[0047] An environment-friendly attapulgite mineral cat litter, comprising the steps of:
[0048] A. Broken
[0049] Break the attapulgite ore;
[0050] B. Raw material preparation
[0051] Attapulgite ore, bentonite ore and additive corn cob powder are prepared by weight, 70 parts of attapulgite ore, 18 parts of bentonite ore, and 18 parts of corn cob powder;
[0052] C. Drying and sieving
[0053] Send the raw materials into a mill and extrude them into granules with a particle size of 2-3mm. Dry them in the air to reduce the moisture content of the attapulgite clay to 15%, then crush them and sieve them to obtain attapulgites. Powder, sieve size is 100-150 mesh;
[0054] D. Baking
[0055] Send the sieved attapulgite powder into a roasting furnace for roasting, the roasting temperature is controlled at 360°C, and the roasting time is 60 minutes to prepare the finished environmental-friendly attapulgite mineral cat litter, and the moisture content in the finished environ...
Embodiment 3
[0057] An environment-friendly attapulgite mineral cat litter, comprising the steps of:
[0058] A. Broken
[0059] Break the attapulgite ore;
[0060] B. Raw material preparation
[0061] Attapulgite ore, bentonite ore and additive rice husk powder are prepared by weight, 75 parts of attapulgite ore, 20 parts of bentonite ore, and 20 parts of rice husk powder;
[0062] C. Drying and sieving
[0063] Send the raw materials into a mill and extrude them into granules with a particle size of 2-3mm. Dry them in the air to reduce the moisture content of the attapulgite clay to 15%, then crush them and sieve them to obtain attapulgites. Powder, sieve size is 100-150 mesh;
[0064] D. Baking
[0065] Send the sieved attapulgite powder into a roasting furnace for roasting, the roasting temperature is controlled at 300°C, and the roasting time is 120 minutes to prepare the finished environmental protection attapulgite mineral cat litter, the moisture content of the finished enviro...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com