Burn-free diatom ecological brick and production method thereof
A technology of ecological bricks and diatoms, applied in the field of decorative materials, can solve the problems of energy pollutant discharge, high construction skill requirements, and high construction costs, and achieve the effects of increasing service life, improving antibacterial and mildew resistance, and saving resources
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0030] Components:
[0031]
[0032]
[0033] Preparation:
[0034] Measure each component except water according to the above ratio, add to the powder mixer, stir for 30 minutes and mix until the powder is uniform.
[0035] Add 54 parts of water into the slurry tank, add the mixed powder under stirring, and stir for 20 minutes until the slurry is uniform after adding the powder.
[0036] Inject the slurry into the prefabricated mold, scrape the top of the mold, and vibrate on the vibration platform.
[0037] Cured for 7 days at a temperature of 15°C-25°C and a relative humidity of 40%-60%, demolded, then cured for 21 days at a temperature of 15°C-25°C and a relative humidity of 40%-60%, and polished.
[0038] After the product has passed the inspection, the finished bricks are pasted on the grid cloth coated with pressure-sensitive adhesive, packed into cartons, and put into storage.
Embodiment 2
[0040] Raw material components:
[0041]
[0042]
[0043] Preparation:
[0044] Measure each component except water according to the above ratio, add to the powder mixer, stir for 30 minutes and mix until the powder is uniform.
[0045] Add 90 parts of water into the pulping tank, add the mixed powder while stirring, and stir for 20 minutes until the slurry is uniform after adding the powder.
[0046] Inject the slurry into the prefabricated mold, scrape the top of the mold, and vibrate on the vibration platform.
[0047] Curing for 7 days at a temperature of 15°C-25°C and a relative humidity of 40%-60%, demoulding, and then curing for 21 days at a temperature of 15°C-25°C and a relative humidity of 40%-60%, demoulding, polished.
[0048] After the product has passed the inspection, the finished bricks are pasted on the grid cloth coated with pressure-sensitive adhesive, packed into cartons, and put into storage.
Embodiment 3
[0050] Raw material components:
[0051]
[0052] Preparation:
[0053] Measure each component except water according to the above ratio, add to the powder mixer, stir for 30 minutes and mix until the powder is uniform.
[0054] Add 30 parts of water into the pulping tank, add the mixed powder while stirring, and stir for 20 minutes until the slurry is uniform after adding the powder.
[0055] Inject the slurry into the prefabricated mold, scrape the top of the mold, and vibrate on the vibration platform.
[0056]Curing for 7 days at a temperature of 15°C-25°C and a relative humidity of 40%-60%, demoulding, and then curing for 21 days at a temperature of 15°C-25°C and a relative humidity of 40%-60%, demoulding, polished.
[0057] After the product has passed the inspection, the finished bricks are pasted on the grid cloth coated with pressure-sensitive adhesive, packed into cartons, and put into storage.
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com