Embodiment 1
[0024] (1) Add 4-2 parts of polyethylene glycol 6000 and 1-2 parts of cetyl alcohol to 6-8 parts of polyethylene oxide, heat to 70-80°C and mix for 5 minutes, then add 1 part of N-methylpyrrolidone and 0.5 parts of benzyltriethylammonium chloride, continue to heat to 110-120 ° C and mix for 10 minutes to obtain material I;
[0025] (2) Add 2-1 parts of polyhydroxyalkanoate and 0.5 parts of tea seed powder to 4-6 parts of activated clay, mix well and let stand for 30 minutes, then heat to 100-110°C and mix for 10 minutes, then add while hot 6-4 parts of maltodextrin and 0.5-1 part of sodium hexametaphosphate are mixed thoroughly to obtain material II;
[0026] (3) Add 30 parts of modified polyvinyl alcohol resin and 4-6 parts of chitosan oligosaccharide to 100-150 parts of water, heat to reflux state and mix for 10 minutes, then add 5-3 parts of pregelatinized potato starch and 2-4 parts Part glutinous rice flour, continue to reflux heat preservation and mix for 10min, obtain ...
Embodiment 2
[0031] (1) Add 4-2 parts of polyethylene glycol 6000 and 1-2 parts of cetyl alcohol to 6-8 parts of polyethylene oxide, heat to 70-80°C and mix for 5 minutes, then add 1 part of N-methylpyrrolidone and 0.5 parts of benzyltriethylammonium chloride, continue to heat to 110-120 ° C and mix for 10 minutes to obtain material I;
[0032] (2) Add 2-1 parts of polyhydroxyalkanoate and 0.5 parts of tea seed powder to 4-6 parts of activated clay, mix well and let stand for 30 minutes, then heat to 100-110°C and mix for 10 minutes, then add while hot 6-4 parts of maltodextrin and 0.5-1 part of sodium hexametaphosphate are mixed thoroughly to obtain material II;
[0033] (3) Add 30 parts of modified polyvinyl alcohol resin and 4-6 parts of chitosan oligosaccharide to 100-150 parts of water, heat to reflux state and mix for 10 minutes, then add 5-3 parts of pregelatinized potato starch and 2-4 parts Part glutinous rice flour, continue to reflux heat preservation and mix for 10min, obtain ...
Embodiment 3
[0038] The performance tests of the pesticide packaging films prepared in Examples 1 and 2 are shown in Table 1.
[0039] The performance test result of the prepared pesticide packaging film in table 1
[0040] Test items Example 1 Example 2 0-5℃ water solubility Completely dissolve within 5s Completely dissolve within 5s 6 months biodegradability 75% 78% 12 months biodegradability 100% 100% 24-month pesticide storage failure rate 0 0
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com