Coating for renovating door head and preparation method of coating
A paint and lintel technology, applied in the field of lintel renovation paint and its preparation, can solve the problems that water-based paint cannot adhere to the smooth lintel surface, increase the process of door lintel renovation, and the sharp deterioration of lintel adhesion, so as to reduce the renovation process , excellent waterproof performance, the effect of less foam
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] Example 1 A paint for door lintel renovation, consisting of the following raw materials in parts by weight: 35 parts of silicon-modified propylene emulsion, 18 parts of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate 30 parts of natural flaky stone powder, 5 parts of multifunctional additives, 7 parts of nano-titanium dioxide, 9 parts of preservatives, 8 parts of dispersants, 4 parts of defoamers, 3 parts of thickeners, and 5 parts of adhesion promoters.
[0018] A method for preparing a coating for door lintel renovation, comprising the following steps:
[0019] (1) Weigh the silicon-modified propylene emulsion, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate and natural flaky stone powder first, start the high-speed mixer, and carry out rapid stirring. Control at 500~600r / min;
[0020] (2) Slowly add multifunctional additives, preservatives, dispersants, defoamers, and thickeners during the stirring process, continue stirring for 12-20 minutes after the addition, and...
Embodiment 2
[0026] Example 2 A paint for lintel renovation, consisting of the following raw materials in parts by weight: 45 parts of silicon-modified propylene emulsion, 24 parts of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate 35 parts, 35 parts of natural flaky stone powder, 15 parts of multifunctional additives, 11 parts of nano-titanium dioxide, 11 parts of preservatives, 10 parts of dispersants, 7 parts of defoamers, 9 parts of thickeners, and 10 parts of adhesion promoters.
[0027] A method for preparing a coating for door lintel renovation, comprising the following steps:
[0028] (1) Weigh the silicon-modified propylene emulsion, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate and natural flaky stone powder first, start the high-speed mixer, and carry out rapid stirring. Control at 500~600r / min;
[0029] (2) Slowly add multifunctional additives, preservatives, dispersants, defoamers, and thickeners during the stirring process, continue stirring for 12-20 minutes after the add...
Embodiment 3
[0035] Example 3 A paint for door lintel renovation, consisting of the following raw materials in parts by weight: 38 parts of silicon-modified propylene emulsion, 22 parts of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate 32 parts, 32 parts of natural flaky stone powder, 12 parts of multifunctional additives, 9 parts of nano-titanium dioxide, 10 parts of preservatives, 9 parts of dispersants, 6 parts of defoamers, 5 parts of thickeners, and 7 parts of adhesion promoters.
[0036] A method for preparing a coating for door lintel renovation, comprising the following steps:
[0037] (1) Weigh the silicon-modified propylene emulsion, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate and natural flaky stone powder first, start the high-speed mixer, and carry out rapid stirring. Control at 500~600r / min;
[0038] (2) Slowly add multifunctional additives, preservatives, dispersants, defoamers, and thickeners during the stirring process, continue stirring for 12-20 minutes after the a...
PUM
| Property | Measurement | Unit |
|---|---|---|
| mechanical properties | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information