[0020] A simulated soft fishing bait is characterized in that: it is made of the following materials by weight,
[0021] 36-40 parts of waste tires, 5-8 parts of waste ceramic powder, 9-12 parts of universal carbon black, 1-3 parts of stearic acid, 1-4 parts of zinc oxide, 2-5 parts of anti-aging agent, 2 parts of pentaerythritol oleate -5 parts, 1-2 parts of molybdenum trioxide, 0.5-1.5 parts of nano tea polyphenols;
[0022] Including the following preparation steps,
[0023] Ⅰ The waste tires are crushed into granules by crushing equipment to remove other impurities except rubber, and then melted into rubber liquid by melting furnace;
[0024] ⅡPut the rubber liquid into a bucket at 62-70°C, and then put in the rest of the materials one by one, one kind every 2 minutes, and stir while putting in;
[0025] Ⅲ After all the materials are put in, continue to stir for 15-20 minutes, let it stand for 5 minutes to cool down naturally, then add 1 / 13 of the total weight of the mat...
Embodiment 2
[0028] A simulated soft fishing bait is characterized in that: it is made of the following materials by weight,
[0029] 40 parts of waste tires, 7 parts of waste ceramic powder, 11 parts of universal carbon black, 1 part of stearic acid, 2 parts of zinc oxide, 3 parts of anti-aging agent, 4 parts of pentaerythritol oleate, 1 part of molybdenum trioxide, nano-tea polyphenol 0.8 copies;
[0030] Including the following preparation steps,
[0031] Ⅰ The waste tires are crushed into granules by crushing equipment to remove other impurities except rubber, and then melted into rubber liquid by melting furnace;
[0032] ⅡPut the rubber liquid into a bucket at 63°C, and then put in the rest of the materials one by one, every 2 minutes, and stir while putting in;
[0033] Ⅲ Continue to stir for 18 minutes after all the materials are put in, let stand for 5 minutes to cool down naturally, then add 1 / 13 of the total weight of the materials in dilute hydrochloric acid solution, and con...
Embodiment 3
[0036] A simulated soft fishing bait is characterized in that: it is made of the following materials by weight,
[0037] 38 parts of waste tires, 6 parts of waste ceramic powder, 9 parts of universal carbon black, 2 parts of stearic acid, 2 parts of zinc oxide, 4 parts of anti-aging agent, 3 parts of pentaerythritol oleate, 1 part of molybdenum trioxide, nano-tea polyphenol 0.1.1 copies;
[0038] Including the following preparation steps,
[0039] Ⅰ The waste tires are crushed into granules by crushing equipment to remove other impurities except rubber, and then melted into rubber liquid by melting furnace;
[0040] ⅡPut the rubber liquid into a bucket at 62°C, and then put in the rest of the materials one by one, every 2 minutes, and stir while putting in;
[0041] Ⅲ Continue to stir for 20 minutes after all the materials are put in, let stand for 5 minutes to cool down naturally, then add 1 / 13 of the total weight of the materials in dilute hydrochloric acid solution, and c...