A method for controlling moisture content of solid wood ecological board
A control method and technology of moisture content, applied in wood compression, wood heating, manufacturing tools, etc., can solve the problems of moisture content change, easy deformation, cracking, etc., achieve moisture stability, reduce cracking and deformation, and change small effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0038] A method for controlling the moisture content of a solid wood ecological board, the method for controlling the moisture content of a solid wood ecological board comprises the following steps:
[0039] a. Treatment of raw wood materials: After felling the raw wood materials, place them for a period of time, peel them off, and leave them in the natural environment for 3 months for pickling, and then process the raw wood materials;
[0040]Among them, the storage period is specifically 20 days,
[0041] b. Cut the raw material into slats: take the processed wood raw material and cut it into slats with a width of 2cm, a length of 40cm, and a thickness of 20mm;
[0042] c. Moisture control of slats: Take the slats and stack them crosswise, push them into the drying room for the first baking, bake until the moisture content of the slats is 19%, and complete the first baking;
[0043] Among them, the temperature of the first baking is 65°C, and the heat source is heat transfe...
Embodiment 2
[0054] A method for controlling the moisture content of a solid wood ecological board, the method for controlling the moisture content of a solid wood ecological board comprises the following steps:
[0055] a. Treatment of raw wood materials: after felling raw wood materials, place them for a period of time, peel them off, and leave them in the natural environment for 6 months for pickling, and then process the raw wood materials;
[0056] Among them, the storage period is specifically 7 days,
[0057] b. cutting the raw materials into slats: take the treated wood raw materials and cut them into slats with a width of 9cm, a length of 60cm and a thickness of 10mm;
[0058] c. Moisture control of slats: Take the slats and stack them crosswise, push them into the drying room for the first baking, bake until the moisture content of the slats is 15%, and complete the first baking;
[0059] Among them, the temperature of the first baking is 78°C, and the heat source is heat transf...
Embodiment 3
[0070] A method for controlling the moisture content of a solid wood ecological board, the method for controlling the moisture content of a solid wood ecological board comprises the following steps:
[0071] a. Treatment of raw wood materials: After felling raw wood materials, place them for a period of time, peel them off, and leave them in a natural environment for 4 months for pickling, and then process the raw wood materials;
[0072] Among them, the storage period is specifically 11 days,
[0073] b. cutting the raw materials into slats: take the processed timber raw materials, the slats are 3cm wide, 45cm long, and 18mm thick.
[0074] c. Moisture control of slats: Take the slats and stack them crosswise, push them into the drying room for the first baking, bake until the moisture content of the slats is 16%, and complete the first baking;
[0075] Among them, the temperature of the first baking is 69°C, and the heat source is heat transfer oil.
[0076] d. Splicing th...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com