preparation example Construction
[0025] figure 2 It is a flow chart of a method for preparing a shell assembly structure according to an embodiment of the present invention. according to figure 2 The shell composite structure prepared by the method shown includes a shell and a plastic bracket, and the plastic bracket is fixed on the shell. The preparation method of the shell composite structure includes:
[0026] Step 101, preparing a shell.
[0027] The preparation method provided in the embodiment of the present invention is used for the preparation of the shell composite structure. The combined housing structure may be a combined housing structure of various terminals, such as mobile phones, wearable devices, and the like.
[0028] The shell combination structure includes a shell and a plastic bracket, wherein the shell can be made of hard materials, such as ceramics, glass, etc., which have the characteristics of high hardness and poor toughness; the plastic bracket is made of plastic materials.
[...
example 1
[0047] 11. Prepare a ceramic shell.
[0048] A mobile phone ceramic shell with a size of 180×90×8 mm is prepared by dry pressing zirconia powder and then sintering. The structure of the prepared mobile phone ceramic shell is as follows image 3 Shown in mark 3.
[0049] 12. Prepare the plastic bracket.
[0050] The injection molding machine injects and molds the plastic bracket of the required structure. The structure of the prepared plastic stent is as follows image 3 Shown in mark 4.
[0051] The injection molding raw material can be Sabic PC1414, the mold temperature of the front and rear molds is 110°C, the injection speed is 120mm / sec, and the pressure is 2800kgf / mm 2 , the cooling time is 6s.
[0052] 13. Dispensing glue.
[0053] Fix the plastic bracket to the jig, and dispense glue on it. The amount of glue is about 7.8g. The amount of glue can be appropriately increased or decreased according to the pulling force and glue overflow.
[0054] 14. Bonding and ma...
example 2
[0072] 21. Prepare a ceramic shell.
[0073] Chaozhou Sanhua zirconia powder was dry-pressed and then sintered to prepare a mobile phone ceramic case with a size of 180×90×8mm.
[0074] 22. Microporous treatment on the surface of the ceramic shell.
[0075] Put the ceramic shell into a special surface treatment tank for microporous corrosion treatment to form nano-scale micropores on the surface of the ceramic shell.
[0076] 23. Insert injection molding to obtain the first product of the composite structure of the ceramic shell.
[0077] Insert injection molding (PBT+30% GF) of the surface-treated ceramic shell, with an injection rate of 280mm / sec and a pressure greater than 2700kgf / mm 2 , so that the plastic bracket is firmly bonded to the ceramic shell, the pulling force can reach more than 80KG, and the first product of the composite structure of the ceramic shell is obtained.
[0078] 24. Annealing.
[0079] Put the primary product of the composite structure of the ce...
PUM