A coating process and flooring technology, which is applied to the device for coating liquid on the surface, the coating, the surface pretreatment, etc., can solve the problems of poor wood grain layering, etc., and achieve enhanced three-dimensional effect, thick color, and three-dimensional antique effect Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] A kind of Grace pattern coating process of wooden floor, concrete steps are as follows:
[0021] (1) Water-based coloring base material, water-based color paste (white) and water-based crosslinking agent are added in a mass ratio of 100:100:3, and continuously stirred by a mechanical mixer for more than 5 minutes until the color is uniform to make a water-based white primer.
[0022] (2) The wooden substrate is sanded by a 180-240 mesh sander. During the sanding process, choose light yarn first and then heavy sand.
[0023] (3) The base material after sanding is directly roller-coated with water-based white primer, and the coating amount is 150-200g / m 2 , and then baked in a 60-80°C hot air infrared drying circulation oven for 1-5min.
[0024] (4) Place the baked base material in a ventilated and cool place to air for 4-24 hours until the cross-linking reaction of the water-based white primer is complete.
[0025] (5) After the base material after the complete reactio...
Embodiment 2
[0032] A kind of Grace pattern coating process of wooden floor, concrete steps are as follows:
[0033] (1) Water-based coloring base material, water-based white color paste and water-based crosslinking agent are added in a mass ratio of 100:100:8, and continuously stirred by a mechanical mixer for more than 5 minutes until the color is uniform to make a water-based white primer.
[0034] (2) Wooden substrates are sanded with 180 mesh and 240 mesh of sanding machine successively.
[0035] (3) The base material after sanding is directly roller-coated with water-based white primer, and the coating amount is 150-200g / m 2 , and then baked in a 60-80°C hot air infrared drying circulation oven for 1-5min.
[0036] (4) Place the baked base material in a ventilated and cool place to air for 4-24 hours until the cross-linking reaction of the water-based white primer is complete.
[0037] (5) After the base material after the complete reaction is lightly polished by a 4-roller Dupont ...
Embodiment 3
[0040] A kind of Grace pattern coating process of wooden floor, concrete steps are as follows:
[0041] (1) Take the wooden substrate coated with water-based primer, lightly sand it with a 4-roller DuPont silk cloth sand machine (700 mesh cloth sand), and use a sponge roller coating and hand rubbing method to apply transparent water with a volume ratio of 1:1. The paint solution after mixing Gliss and water-based Gliss colorant evenly is coated on the water-based white primer, and the coating amount is 40-60g / m 2 , 60-80 ℃ hot air infrared drying circulation oven drying 15-20s.
[0042] (2) Apply adhesion primer and high-definition topcoat sequentially on the substrate, and the coating amount is 15-20g / m 2 , UV irradiation after coating, the energy density is 110-140mJ / cm 2 .
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com