Embodiment 1
[0027] Take 5 parts of deionized water, 3 parts of edible alcohol, 30 parts of styrene copolymer, 40 parts of acrylic resin, and 1 part of auxiliary agent.
[0028] Based on the above-mentioned raw materials in parts by weight ratio, the implementation plan provided is: the production process of an environmentally friendly water-based coating that ensures the smoothness of cigarette wrapping paper printing, including the following steps:
[0029] Step 1: Take 5 parts of deionized water and 3 parts of edible alcohol in sequence and mix them in the dispersing kettle, and disperse at a uniform speed for 15 minutes at a speed of 300-350 rpm; The rotation speed is dispersed for another 10 minutes and can be reserved for use;
[0030] Step 2: Take 40 parts of acrylic resin, 30 parts of styrene copolymer, and 0.5 parts of high-density polyethylene wax dispersion additive in sequence and mix them in the dispersion kettle, and perform high-speed dispersion for 20 minutes at a speed of ...
Embodiment 2
[0032] Take 10 parts of deionized water, 5 parts of edible alcohol, 40 parts of styrene copolymer, 60 parts of acrylic resin, and 5 parts of additives.
[0033] Based on the above-mentioned raw materials in parts by weight ratio, the implementation plan provided is: the production process of an environmentally friendly water-based coating that ensures the smoothness of cigarette wrapping paper printing, including the following steps:
[0034] Step 1: Take 10 parts of deionized water and 5 parts of edible alcohol in sequence and mix them in the dispersing kettle, and disperse at a uniform speed for 15 minutes at a speed of 300-350 rpm; then add 2 parts of defoaming additives and continue The rotation speed is dispersed for another 10 minutes and can be reserved for use;
[0035] Step 2: Take 60 parts of acrylic resin, 40 parts of styrene copolymer, and 2 parts of high-density polyethylene wax dispersion additives in sequence and mix them in the dispersion kettle, and perform hi...
Embodiment 3
[0037] Take 8 parts of deionized water, 4 parts of edible alcohol, 35 parts of styrene copolymer, 50 parts of acrylic resin, and 3 parts of additives.
[0038] Based on the above-mentioned raw materials in parts by weight ratio, the implementation plan provided is: the production process of an environmentally friendly water-based coating that ensures the smoothness of cigarette wrapping paper printing, including the following steps:
[0039] Step 1: Take 8 parts of deionized water and 4 parts of edible alcohol in turn and mix them in the dispersing kettle, and disperse at a uniform speed for 15 minutes at a speed of 300-350 rpm; then add 1 part of defoaming aid and continue The rotation speed is dispersed for another 10 minutes and can be reserved for use;
[0040] Step 2: Take 50 parts of acrylic resin, 35 parts of styrene copolymer, and 1 part of high-density polyethylene wax dispersion additive in sequence and mix them in a dispersion kettle, and perform high-speed dispersi...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com