Production process for paper
A production process and paper technology, applied in the field of paper manufacturing, can solve the problems of resource waste, low utilization rate of waste paper, insufficient whiteness, etc., and achieve the effects of reducing waste paper waste, improving recycling rate, and maintaining smoothness
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0042] A paper production process, comprising the steps of:
[0043] S1. Classify the waste paper, put the classified paper into the beater, and inject water into the beater, and then perform beating for 35 minutes, so that the paper is dissolved into a slurry;
[0044] S2, pumping the slurry in step S1 to the inclined screen for slurry filtration;
[0045] S3, separating fibers from the slurry filtered in step S2 through a fiber separator to obtain pulp fibers;
[0046] S4. Add wood fiber to step S3, and stir and mix wood fiber and pulp fiber, and the percentage of wood fiber and pulp fiber is 1:3;
[0047] S5. Add talcum powder and calcium carbonate to the stirred slurry, and stir until uniform. The stirring time is 20 minutes, and the particle size of the talcum powder is 1800 mesh;
[0048] S6, add barium sulfate and rosin in step S2, and stir 5min;
[0049] S7. Pump the slurry in step S3 to the slurry distribution equipment, spray the slurry onto the forming net throug...
Embodiment 2
[0057] A paper production process, comprising the steps of:
[0058] S1. Classify the waste paper, put the classified paper into the beater, and inject water into the beater, and then perform beating for 50 minutes, so that the paper is dissolved into a slurry;
[0059] S2, pumping the slurry in step S1 to the inclined screen for slurry filtration;
[0060] S3, separating fibers from the slurry filtered in step S2 through a fiber separator to obtain pulp fibers;
[0061] S4. Add wood fiber to step S3, and stir and mix wood fiber and pulp fiber, and the percentage of wood fiber and pulp fiber is 1:5;
[0062] S5. Add talcum powder and calcium carbonate to the stirred slurry, and stir until uniform. The stirring time is 32 minutes, and the particle size of the talcum powder is 2300 mesh;
[0063] S6, add barium sulfate and rosin in step S2, and stir 10min;
[0064] S7. Pump the slurry in step S3 to the slurry distribution equipment, spray the slurry onto the forming net throu...
Embodiment 3
[0072] A paper production process, comprising the steps of:
[0073] S1. Sorting the waste paper, putting the sorted paper into the beater, and injecting water into the beater, and then beating for 65 minutes, so that the paper is dissolved into a slurry;
[0074] S2, pumping the slurry in step S1 to the inclined screen for slurry filtration;
[0075] S3, separating fibers from the slurry filtered in step S2 through a fiber separator to obtain pulp fibers;
[0076] S4. Add wood fiber to step S3, and stir and mix wood fiber and pulp fiber, and the percentage of wood fiber and pulp fiber is 1:6;
[0077] S5. Add talcum powder and calcium carbonate to the stirred slurry, and stir until uniform. The stirring time is 44 minutes, and the particle size of the talcum powder is 2600 mesh;
[0078] S6, add barium sulfate and rosin in step S2, and stir 15min;
[0079] S7. Pump the slurry in step S3 to the slurry distribution equipment, spray the slurry onto the forming net through the...