[0033] Composition of seashore titanium sand rough concentrate: TiO 2 42.20%, Fe 38.76%, CaO 0.20%, MgO 0.62%, Al 2 o 3 0.82%, SiO 2 2.29%.
[0034] Above-mentioned raw ore is passed through following processing steps:
[0035] (1) Add 15% reduced carbon powder and mix evenly with titanium coarse concentrate, use rotary kiln equipment to carry out reduction roasting, the roasting temperature is 875 ° C, and the reduction roasting time is 55 minutes to obtain calcined sand;
[0036] (2) The calcined sand obtained by reduction roasting is cooled by water quenching, and then the excessive reducing agent in the calcined sand is recovered by a shaking table gravity separation process, and heavy sand is obtained;
[0037] (3) The heavy sand is separated by a two-stage weak magnetic separation process, the strength of the weak magnetic separation rough separation is 0.15T, and the iron coarse concentrate 1 is obtained, and the rough separation tailings are subjected to weak magne...
Embodiment 2
[0042] Composition of seashore titanium sand rough concentrate: TiO 2 : 43.07%, Fe: 41.47%, CaO: 0.18%, MgO: 0.51%, Al 2 o 3 : 0.83%, SiO 2: 1.85%.
[0043] Above-mentioned raw ore is passed through following processing steps:
[0044] (1) Add 25% reduced carbon powder and titanium coarse concentrate and mix evenly, and use rotary kiln equipment to carry out reduction roasting, the roasting temperature is 750 ° C, and the reduction roasting time is 85 minutes to obtain calcined sand;
[0045] (2) The calcined sand obtained by reduction roasting is cooled by water quenching, and then the excessive reducing agent in the calcined sand is recovered by a spiral chute gravity separation process, and heavy sand is obtained;
[0046] (3) The heavy sand is separated by two-stage weak magnetic separation process, the strength of weak magnetic rough separation is 0.10T, and iron coarse concentrate 1 is obtained. The strength is 0.30T, and the iron coarse concentrate 2 and titanium c...