Method for making safe latex products with fragrance and medicinal plants added
The technology of a latex product and a production method is applied in the production field of safe latex products, and can solve the problems of poor air permeability, high hardness of latex pillows, affecting the use of latex pillows, etc., and achieve the effects of good elasticity, good antibacterial performance, and good elasticity.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0082] S1: Mixing, uniformly mix 120 parts of natural latex, 2 parts of wormwood, and 1 part of saponin powder with a particle size of 20nm, and add soda until the pH value of the mixture is 9.5; wherein, the water content of natural latex is 35% ;
[0083] S2: Injection molding, filling the uniformly mixed mixture into the mold;
[0084] S3: Vacuum foaming, vacuum foam the mixture in the mold after closing the mold, the pressure in the cavity is 20Pa, and keep it for 40min;
[0085] S4: freeze and solidify, lower the temperature inside the mold to -25°C, and keep it for 10 minutes;
[0086] S5: Forming, raising the temperature inside the mold to 105°C and maintaining it for 15 minutes;
[0087] S6: Rinse, rinse the latex pillow that has been cooled and solidified with water;
[0088] S7: drying, drying the rinsed latex pillow in an oven at 40° C. for 6 hours.
Embodiment 2
[0090] S1: Mixing, uniformly mix 120 parts of natural latex, 2 parts of wormwood, and 1 part of saponin powder with a particle size of 30nm, and add soda until the pH value of the mixture is 10; wherein, the water content of natural latex is 40% ;
[0091] S2: Injection molding, filling the uniformly mixed mixture into the mold;
[0092] S3: Vacuum foaming. After the mold is closed, the mixture in the mold is vacuum foamed. The pressure in the cavity is 30Pa and kept for 50min;
[0093] S4: freeze and solidify, lower the temperature inside the mold to -28°C, and keep it for 13 minutes;
[0094] S5: Forming, raising the temperature inside the mold to 110°C and maintaining it for 18 minutes;
[0095] S6: Rinse, rinse the latex pillow that has been cooled and solidified with water;
[0096]S7: drying, drying the rinsed latex pillow in an oven at 50° C. for 7 hours.
Embodiment 3
[0098] S1: Mixing, uniformly mix 120 parts of natural latex, 2 parts of wormwood, and 1 part of saponin powder with a particle size of 40nm, and add soda until the pH value of the mixture is 10.5; wherein, the water content of natural latex is 45% ;
[0099] S2: Injection molding, filling the uniformly mixed mixture into the mold;
[0100] S3: Vacuum foaming, vacuum foaming the mixture in the mold after closing the mold, the pressure in the cavity is 40Pa, and keep it for 60min;
[0101] S4: freeze and solidify, lower the temperature inside the mold to -30°C, and keep it for 15 minutes;
[0102] S5: Forming, raising the temperature inside the mold to 120°C and maintaining it for 20 minutes;
[0103] S6: Rinse, rinse the latex pillow that has been cooled and solidified with water;
[0104] S7: drying, drying the rinsed latex pillow in an oven at 60° C. for 8 hours.
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle diameter | aaaaa | aaaaa |
| particle diameter | aaaaa | aaaaa |
| particle diameter | aaaaa | aaaaa |