Embodiment 1
[0026] A heat-stable indoor discharge smokeless and sulfur-free cold fireworks agent, the mass percentage of each component is as follows:
[0027]
[0028] Take 23.47g of nitrobamboo cellulose powder and divide it into two groups, A and B, wherein 7.47g of group A and 16g of group B, and dissolve the nitrobamboo cellulose powder of group A in 74.7g of ethyl acetate, and stir under the condition of ultrasonic dispersion 2.3 hours, then continue under stirring state, add 5.59g polyethylene wax powder and 11.63g zinc stearate powder, stir well, make nitrocellulose mixed sol;
[0029] Add 40g of pentaerythritol tetranitrate powder and 2.96g of titanate coupling agent to 400g of acetone, and ultrasonically disperse for 42 minutes to obtain a mixed solution C; transfer the mixed solution C to an ice-water bath for stirring; then add 0.83g of polyethylene Add the alcohol butyral adhesive to the mixed solution C and stir for 3.7 hours; transfer the reaction device to an oil bath a...
Embodiment 2
[0036] A heat-stable indoor discharge smokeless and sulfur-free cold fireworks agent, the mass percentage of each component is as follows:
[0037]
[0038]
[0039] Take 6.82kg of nitrobamboo cellulose powder and divide it into two groups, A and B, wherein 1.82kg of group A and 5kg of group B, and dissolve the nitrobamboo cellulose powder of group A in 18.2kg of ethyl acetate, and stir under the condition of ultrasonic dispersion 2.7 hours, then continue under stirring state, add 1.29kg polyethylene wax powder and 2.09kg zinc stearate powder, stir, make nitrocellulose mixed sol;
[0040] Add 13kg of pentaerythritol tetranitrate powder and 0.91kg of titanate coupling agent to 130kg of acetone and disperse ultrasonically for 38 minutes to obtain mixed solution C; transfer mixed solution C to an ice-water bath for stirring; then add 0.28kg of polyethylene Add the alcohol butyral adhesive to the mixed solution C and stir for 4.2 hours; transfer the reaction device to an oil b...
Embodiment 3
[0047] A heat-stable indoor discharge smokeless and sulfur-free cold fireworks agent, the mass percentage of each component is as follows:
[0048]
[0049]
[0050] Take 26.13kg of nitrobamboo cellulose powder and divide it into two groups, A and B, wherein group A is 8.13kg and group B is 18kg, and the nitrocellulose powder of group A is dissolved in 81.3kg of ethyl acetate, and stirred under the condition of ultrasonic dispersion 2.3 hours, then continue under stirring state, add 6.28kg polyethylene wax powder and 16.55kg zinc stearate powder, stir evenly, make nitrocellulose mixed sol;
[0051] Add 66kg of pentaerythritol tetranitrate powder and 4.62kg of titanate coupling agent to 660kg of acetone, and ultrasonically disperse for 50 minutes to obtain a mixed solution C; transfer the mixed solution C to an ice-water bath for stirring; then add 1.34kg of polyethylene Add the alcohol butyral adhesive to the mixed solution C and stir for 3.5 hours; transfer the reaction...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com