A coating and wall technology, applied in the field of wall coating and its preparation, can solve the problems of environmental protection and functional defects of traditional materials, and achieve the advantages of being beneficial to large-scale output, enhancing the rheological bonding effect, and being simple and easy to operate. control effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0031] The present embodiment provides a kind of preparation method of wall coating, comprises the steps:
[0032] (1) In the first container, add 200g bitter soil, 130g aluminum silicate powder, 110g zeolite powder, 80g ceramic powder, 80g fire sandstone, 50g bauxite, 30g medical stone, 5g strange ice stone and 3g ice long Stone, under the condition of 80r / min, stirred for 30min to obtain the first mixture;
[0033] (2) In the second container, add 40g of glass powder, 40g of pearl powder, 18g of latex powder and 15g of pregelatinized starch, and stir for 20min under the condition of 100r / min to obtain the second mixture;
[0034] (3) In the third container, add 5g of hydroxyethyl cellulose, 3g of amylase, 2g of vegetable protein and 2g of polypropylene anti-cracking fiber, and stir for 5min under the condition of 40r / min to obtain the third mixture;
[0035] (4) Add the first mixture, the second mixture, and the third mixture into the same container for mixing, and finally ...
Embodiment 2
[0037] The present embodiment provides a kind of preparation method of wall coating, comprises the steps:
[0038] (1) In the first container, add 250g bitter soil, 170g aluminum silicate powder, 140g zeolite powder, 130g ceramic powder, 120g fire sandstone, 100g bauxite, 60g medical stone, 10g strange ice stone and 7g ice Stone, under the condition of 100r / min, stirred for 40min to obtain the first mixture;
[0039] (2) In the second container, add 70g of glass powder, 60g of pearl powder, 25g of latex powder and 30g of pregelatinized starch, and stir at 120r / min for 30min to obtain the second mixture;
[0040] (3) In the third container, add 10g of hydroxyethyl cellulose, 7g of amylase, 5g of vegetable protein and 5g of polypropylene anti-cracking fiber, and stir for 10min under the condition of 60r / min to obtain the third mixture;
[0041] (4) Add the first mixture, the second mixture, and the third mixture into the same container for mixing, and finally add water and cont...
Embodiment 3
[0043] The present embodiment provides a kind of preparation method of wall coating, comprises the steps:
[0044] (1) In the first container, add 225g bitter soil, 150g aluminum silicate powder, 125g zeolite powder, 105g ceramic powder, 100g fire sandstone, 75g bauxite, 45g medical stone, 7g strange ice stone and 5g ice Stone, under the condition of 90r / min, stirred for 35min to obtain the first mixture;
[0045] (2) In the second container, add 55g of glass powder, 50g of pearl powder, 21g of latex powder and 22g of pregelatinized starch, and stir for 25min under the condition of 110r / min to obtain the second mixture;
[0046](3) In the third container, add 7g of hydroxyethyl cellulose, 5g of amylase, 3g of vegetable protein and 3g of polypropylene anti-cracking fiber, and stir for 7min under the condition of 50r / min to obtain the third mixture;
[0047] (4) Add the first mixture, the second mixture, and the third mixture into the same container for mixing, and finally add ...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
particle size | aaaaa | aaaaa |
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com