Preparation method of zinc chloride modified red mud
A technology of zinc chloride and red mud, applied in the field of chemistry, can solve the problem of low phosphorus removal adsorption capacity of red mud, and achieve the effects of short synthesis processing time, stable quality and uniform appearance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0019] The method for preparing zinc chloride modified red mud by constant temperature stirring method, the steps are as follows:
[0020] (1) Select 5g of red mud passed through a 100-mesh sieve and place it in a 250mL triangular round bottom flask, add 100mL0.3mol / LZnCl 2 solution,
[0021] (2) Place the above flask in the HH.S precision constant temperature water bath generator, adjust the water temperature in the water bath to 30°C (ie modification temperature), and stir and react at constant temperature for 1h (ie modification time);
[0022] (3) The solid phase obtained after suction filtration of the reaction solution is zinc chloride modified red mud, and the zinc chloride modified red mud is washed with distilled water until the filtrate does not contain chloride ions (detection: drop 0.1mol / L of silver nitrate to No white precipitate is formed), dried at 105°C, ground, and passed through a 100-mesh sieve to prepare a zinc chloride-modified red mud product.
Embodiment 2-10
[0023] Embodiment 2-10: The preparation steps are the same as in Example 1, except that the ZnCl in the step (1) 2 Concentration, modification temperature and modification time in step (2), see Table 1 for details.
[0024] Each 0.2 g of zinc chloride modified red mud products prepared in the above examples is used to simulate the adsorption treatment of phosphorus-containing wastewater. The experimental method is a conventional method in the art, as follows:
[0025] Weigh 0.2197g KH 2 PO 4 (analytical pure), dissolved in deionized water, transferred to a 1000ml volumetric flask and constant to the mark with deionized water, to obtain a phosphoric acid solution with a concentration of 50mg / L.
[0026] The prepared modified zinc chloride red mud was used as an adsorbent to treat the above-mentioned simulated phosphorus-containing wastewater, and the static method was used for testing: adjust the pH value of the phosphoric acid solution to 3.0, and take 50 mg / L of KH 2 PO 4...
PUM
Login to View More Abstract
Description
Claims