A technology of optical diffusion and composition, which is applied in the field of liquid crystal display devices and optical diffusion films, can solve the problems of ozone layer destruction, environmental pollution, physical injury of R&D and production personnel, etc., and achieve the effect of proper viscosity change and good dispersibility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0056] Embodiment 1: the preparation of composition 1
[0057] (1) Prepare 186.50 parts by weight of solvent, specifically adding 33.05 parts by weight of methyl ethyl ketone (Ningbo Chemical Materials Co., Ltd.), 54.85 parts by weight of butyl acetate (Ningbo Chemical Materials Co., Ltd.), 98.60 parts by weight of Ethyl acetate (Ningbo Chemical Raw Materials Co., Ltd.), cover the lid for subsequent use.
[0058] (2) Add 36.50 parts by weight of particle filler PMMA (MBX-20, Japan Sekisui Chemical Co., Ltd.) in container 002, the particle size is 1-100 microns, then the solvent in the above-mentioned container 001 is added to the container step by step In 002, use a stainless steel rod to slowly disperse the granular filler until all the solvent in the container 001 is added, and then put the container 002 on the stirrer (DJ660, Wuxi Deaosay Mixing Equipment Co., Ltd.) to stir, and the number of revolutions of the stirrer is 2000r / min, stop stirring after 10min.
[0059] (3)...
Embodiment 2
[0061] Embodiment 2: the preparation of composition 2
[0062] (1) Prepare 186.50 parts by weight of solvent, specifically adding 54.85 parts by weight of methyl ethyl ketone (Ningbo Chemical Materials Co., Ltd.), 33.05 parts by weight of butyl acetate (Ningbo Chemical Materials Co., Ltd.), 98.60 parts by weight of Ethyl acetate (Ningbo Chemical Raw Materials Co., Ltd.), cover the lid for subsequent use.
[0063] (2) Add 36.50 parts by weight of particle filler PMMA (MBX-20, Japan Sekisui Chemical Co., Ltd.) in container 002, the particle size is 1-100 microns, then the solvent in the above-mentioned container 001 is added to the container step by step In 002, use a stainless steel rod to slowly disperse the granular filler until all the solvent in the container 001 is added, and then put the container 002 on the stirrer (DJ660, Wuxi Deaosay Mixing Equipment Co., Ltd.) to stir, and the number of revolutions of the stirrer is 2000r / min, stop stirring after 10min.
[0064] (3)...
Embodiment 3
[0066] Embodiment 3: the preparation of composition 3
[0067] (1) Prepare 186.50 parts by weight of solvent, specifically adding 54.85 parts by weight of methyl ethyl ketone (Ningbo Chemical Materials Co., Ltd.), 54.85 parts by weight of butyl acetate (Ningbo Chemical Materials Co., Ltd.), 76.80 parts by weight of Ethyl acetate (Ningbo Chemical Raw Materials Co., Ltd.), cover the lid for subsequent use.
[0068] (2) Add 36.50 parts by weight of particle filler PMMA (MBX-20, Japan Sekisui Chemical Co., Ltd.) in container 002, the particle size is 1-100 microns, then the solvent in the above-mentioned container 001 is added to the container step by step In 002, use a stainless steel rod to slowly disperse the granular filler until all the solvent in the container 001 is added, and then put the container 002 on the stirrer (DJ660, Wuxi Deaosay Mixing Equipment Co., Ltd.) to stir, and the number of revolutions of the stirrer is 2000r / min, stop stirring after 10min.
[0069] (3)...
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle diameter | aaaaa | aaaaa |
| hardness | aaaaa | aaaaa |
| particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 