Surface color-fixing dye for mat rush products, preparation method and color-fixing method
A product, rush technology, applied in the field of preparation of the color-fixing dye, can solve the problems of reducing the degree of dust pollution, not reducing the amount of dyed soil, and the difficulty of popularizing organic complexes, so as to achieve long-lasting retention time, convenient adjustment, and high color and luster. better plumping effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] The content of each component in the slurry (mass percentage):
[0030] Polyvinyl acetate: 15%;
[0031] TiO 2 (average particle size 0.5μm): 4%;
[0032] Dyeing additive (phthalocyanine green, average particle size 0.2μm): 2%;
[0033] Water: balance.
[0034] Add the above components into water in turn while stirring mechanically in proportion to prepare 2kg of slurry, and use electrostatic spraying method to coat the surface of rush mat that has been dyed and fixed with soil, and then enter the hot air drying tunnel. Cured at 80°C for 6 minutes. During the coating process, the slurry in the tank should not stop stirring to ensure the uniformity and stability of the slurry. Before spraying, the surface of rush mat has a light green color and poor color consistency. After spraying and curing, the mat has good uniformity and full color.
Embodiment 2
[0036] The content of each component in the slurry (mass percentage):
[0037] Polyvinyl acetate: 16%;
[0038] TiO 2 : 3% (average particle size 0.9μm);
[0039] Dyeing additive (phthalocyanine green, average particle size 0.5μm): 1%,
[0040] Water: balance.
[0041] Add the above components to water in turn while stirring mechanically in proportion to prepare 5kg of paint, and use the method of electrostatic spraying to paint on the surface of rush grass mat that has been dyed and fixed with soil, and then enter the drying tunnel at 85°C Cured for 5 minutes. During the painting process, the paint in the bucket should not stop stirring to ensure the uniformity of the paint. Before spraying, the surface of the rush mat has a slightly lighter green color and poor gloss. After the above slurry is sprayed and cured, the apparent color of the mat is uniform and full, which improves the apparent color quality of the rush mat.
Embodiment 3
[0043] The content of each component in the slurry (mass percentage):
[0044] Polyvinyl acetate: 18%;
[0045] TiO 2 : 2% (average particle size 0.6μm);
[0046]Dyeing additive (chlorophyll): 0.1%,
[0047] Water: balance.
[0048] Add the above components to water in turn while stirring mechanically in proportion to prepare 5kg of paint, and use the method of electrostatic spraying to paint on the surface of rush grass mat that has been dyed and fixed with soil, and then enter the drying tunnel at 85°C Cured for 5 minutes. During the painting process, the paint in the bucket should not stop stirring to ensure the uniformity of the paint. Before spraying, the surface of the rush mat has a slightly lighter green color and poor gloss. After the above slurry is sprayed and cured, the apparent color of the mat is uniform and full, which improves the apparent color quality of the rush mat.
PUM
Property | Measurement | Unit |
---|---|---|
The average particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information

- Generate Ideas
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com