Self-activation flotation method for component of fluid inclusion of copper sulfide ore
A technology for fluid inclusions and copper sulfide ore, which is used in flotation, solid separation and other directions to reduce the cost of flotation, reduce the amount of collectors, and reduce the amount of use.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0024] The copper sulfide ore contains 0.70% copper, and the oxidation rate is 8%. The copper sulfide mineral is chalcopyrite, the copper oxide mineral is malachite, the ore type is hydrothermal type, and the fluid inclusions are rich.
[0025] (1) The ore is ground at a concentration of 80-85wt% until the dissociation degree of the copper sulfide mineral monomer is greater than 80%, the grinding fineness is -200 mesh and the content reaches 88%. The copper in the fluid inclusions of the copper sulfide mineral Ions are released into the slurry solution while the newly formed surface of the copper sulfide mineral relaxes to form a "sulfur-rich" surface.
[0026] (2) Dilute the copper sulfide ore grinding slurry obtained in step (1) with water to a concentration of 30wt%, add 60g / t ammonium chloride, put it into the first sealed mixing tank, and slow down at a speed of 0.5-1m / s Stir at high speed, so that the copper ions released from the fluid inclusions and the added copper io...
Embodiment 2
[0030] The copper sulfide ore contains 0.90% copper, and the oxidation rate is 10%. The copper sulfide mineral is mainly chalcopyrite, followed by chalcocite, the copper oxide mineral is malachite, the ore type is hydrothermal type, and the fluid inclusions are rich.
[0031] (1) The ore is ground at a concentration of 80-85wt% until the dissociation degree of the copper sulfide mineral monomer is greater than 80%, the grinding fineness is -200 mesh and the content reaches 90%. The copper in the fluid inclusions of the copper sulfide mineral Ions are released into the slurry solution while the newly formed surface of the copper sulfide mineral relaxes to form a "sulfur-rich" surface.
[0032] (2) Dilute the copper sulfide ore grinding slurry obtained in step (1) with water to a concentration of 35wt%, add 70g / t of ammonium chloride, put it into the first sealed mixing tank, and slow down at a speed of 0.5-1m / s Stir at high speed, so that the copper ions released from the fluid...
Embodiment 3
[0036] Copper sulfide ore contains 1.10% copper grade and 12% oxidation rate. The copper sulfide mineral is mainly chalcopyrite, followed by bornite. The copper oxide mineral is malachite. The ore type is hydrothermal metamorphic type with fluid inclusions , but less than the hydrothermal type.
[0037] (1) The ore is ground at a concentration of 80-85wt% until the dissociation degree of the copper sulfide mineral monomer is greater than 80%, the grinding fineness is -200 mesh and the content reaches 85%. The copper in the fluid inclusions of the copper sulfide mineral Ions are released into the slurry solution while the newly formed surface of the copper sulfide mineral relaxes to form a "sulfur-rich" surface.
[0038] (2) Dilute the copper sulfide ore grinding slurry obtained in step (1) with water to a concentration of 40wt%, add 5 (or 8, or 10) g / t of copper sulfate, add 100 g / t of ammonium chloride, and put it into the A sealed mixing tank is stirred at a slow speed of 0...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com