Embodiment 1
[0024] A preparation method of an environment-friendly water-based two-component automotive refinish paint primer, the method comprising the following process steps:
[0025] (1) First add water-based resin (Bayhydrol A 145) 35%, water-based wetting agent (Surfynol 104BC) 0.8%, water-based dispersant (TEGO Dispers 715W) 1.3%, water-based corrosion inhibitor (SER-AD FA 179) 0.4%, Calcium carbonate 41%, deionized water 11.5% were added sequentially under stirring and mixed evenly for 10 minutes, then ground to a fineness of less than 20um to prepare component A;
[0026] (2) 8% of polyisocyanate resin (Bayhydrol XP 304) and 2% of solvent (butyl acetate) were added in sequence and stirred evenly; component B was obtained.
[0027] Components A and B are used after mixing evenly during construction.
Embodiment 2
[0029] A preparation method of an environment-friendly water-based two-component automotive refinish paint primer, the method comprising the following process steps:
[0030] (1) Water-based resin (Bayhydrol A 2546) 38%, water-based wetting agent (Surfynol 104BC) 0.7%, water-based dispersant (TEGO Dispers 740W) 1.4%, water-based corrosion inhibitor (SER-AD FA 179) 0.4%, 38% titanium dioxide and 11.5% deionized water were added in sequence under stirring and mixed evenly for 10 minutes, then ground to a fineness of less than 20um to prepare component A;
[0031] (2) 8% of polyisocyanate resin (Bayhydrol XP 304) and 2% of solvent (butyl acetate) were added in sequence and stirred evenly; component B was obtained.
[0032] Components A and B are used after mixing evenly during construction.
Embodiment 3
[0034] A preparation method of an environment-friendly water-based two-component automotive refinish paint primer, the method comprising the following process steps:
[0035] (1) First add water-based resin (Bayhydrol A 2227 / 1) 37%, water-based wetting agent (Surfynol 104BC) 0.6%, water-based dispersant (TEGO Dispers 745W) 1.5%, water-based corrosion inhibitor (SER-AD FA 179) 0.4 %, calcium carbonate 39%, and deionized water 11.5% were added in sequence under stirring and mixed evenly for 10 minutes, then ground to a fineness of less than 20um to prepare component A;
[0036] (2) 8% of polyisocyanate resin (Bayhydrol desmodur 3100) and 2% of solvent (butyl acetate) were added in sequence and stirred evenly; component B was obtained.
[0037] Components A and B are used after mixing evenly during construction.