Embodiment 1
[0022] The water-based gold ink raw material formula of the present embodiment is as follows:
[0023] 25 parts copper gold powder;
[0024] 35 parts of alcohol water-based polyurethane;
[0025] 15 parts of alcohol;
[0026] 10 parts of water;
[0027] Coconut oil monoethanolamide 0.5 parts.
[0028] Prepare the water-based gold ink of this example as follows: dissolve 0.5 parts of coconut oil monoethanolamide in 10 parts of water, then immerse 25 parts of copper and gold powder in it for wetting, add 15 parts of alcohol and 35 parts of alcohol after 30 minutes Water-based polyurethane, stir well; test color and viscosity afterwards.
[0029] The surface color of the water-based gold ink prepared in this example is red-gold, and the copper powder does not turn green.
[0030] According to GB / T13217.7-2009 [Test method for liquid ink adhesion fastness], the adhesion fastness is 95%, which is similar to ordinary solvent-based gold ink of the same color.
[0031] Evaluatio...
Embodiment 2
[0033] The water-based gold ink raw material formula of the present embodiment is as follows:
[0034] 30 parts copper gold powder;
[0035] 35 parts of alcohol water-based polyurethane;
[0036] Alcohol 25 parts;
[0037] 25 parts of water;
[0038] Coconut oil monoethanolamide 1.5 parts.
[0039] Prepare water-based gold ink as follows: dissolve 1.5 parts of coconut oil monoethanolamide in 25 parts of water, then immerse 30 parts of copper and gold powder in it for wetting, add 25 parts of alcohol and 35 parts of alcohol water-based polyurethane after 30 minutes, and stir Uniform; test color and viscosity afterwards.
[0040] The surface color of the water-based gold ink prepared in this example is red-gold, and the copper powder does not turn green.
[0041] According to GB / T13217.7-2009 [Test method for liquid ink adhesion fastness], the adhesion fastness is level 5, which is similar to ordinary solvent-based gold ink of the same color.
[0042] Evaluation of the use...
Embodiment 3
[0044] The water-based gold ink raw material formula of the present embodiment is as follows:
[0045] 28 parts copper gold powder;
[0046] 48 parts of alcohol water-based polyurethane;
[0047] 20 parts of alcohol;
[0048] 15 parts of water;
[0049] Coconut Oil Monoethanolamide 1 part.
[0050] Prepare water-based gold ink as follows: dissolve 1 part of coconut oil monoethanolamide in 15 parts of water, then immerse 28 parts of copper and gold powder in it for wetting, add 20 parts of alcohol and 48 parts of alcohol water-based polyurethane after 30 minutes, and stir Uniform; test color and viscosity afterwards.
[0051] The surface color of the water-based gold ink prepared in this example is red-gold, and the copper powder does not turn green.
[0052] According to GB / T13217.7-2009 [Test method for liquid ink adhesion fastness], the adhesion fastness is level 5, which is similar to ordinary solvent-based gold ink of the same color.
[0053] Evaluation of the use ef...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com