High-resolution water-based flexible printing ink and preparation method thereof
A high-resolution, ink technology, applied in the field of high-resolution water-based flexographic ink and its preparation, can solve the problems of not being able to reflect the three-dimensional effect, difficult to clearly express complex graphics, etc. thin effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] (1) Add 20 parts of water-based acrylic resin, 30 parts of pigment, 2 parts of dispersant 760W produced by Dow Corning, 20 parts of water, 10 parts of ethanol and 1 part of defoamer into a high-speed mixer for pre-dispersion, and the stirring speed is controlled by a frequency conversion motor , Stir slowly first to avoid the slurry from spilling out, then stir at a high speed of 1000-2000 rpm to make the mixture even;
[0023] (2) Put the pre-dispersed slurry into the sand mill for sanding; the particle size of the sanded slurry is less than 10um.
[0024] (3) Add acrylic emulsion to the slurry after sanding, in which the mass of acrylic emulsion accounts for 20%, and the mass of slurry accounts for 70%. Stir and mix evenly, and add solvent at the same time so that the viscosity of the ink is Tu 4 Viscosity Cup 20 -30s, the solvent is water and ethanol, and the volume ratio of water and ethanol is 2:1. The prepared ink has excellent pigment dispersibility and good sta...
Embodiment 2
[0026] (1) Add 30 parts of water-based acrylic resin, 60 parts of pigment, 8 parts of dispersant 760W produced by Dow Corning, 15 parts of water, 10 parts of ethanol and 0.5 part of defoamer into a high-speed mixer for pre-dispersion, and the stirring speed is controlled by a frequency conversion motor , Stir slowly first to avoid the slurry from spilling out, then stir at a high speed of 1000-2000 rpm to make the mixture even;
[0027] (2) Put the pre-dispersed slurry into the sand mill for sanding; the particle size of the sanded slurry is less than 10um.
[0028] (3) Add acrylic emulsion to the slurry after sanding, wherein the amount of acrylic emulsion is 30%, the amount of slurry is 60%, stir and mix evenly, and add solvent at the same time so that the viscosity of the ink is Tu 4 viscosity cup 20 -30s, the solvent is water and ethanol, and the volume ratio of water and ethanol is 1:1. The prepared ink has excellent pigment dispersibility and good stability, and the ink...
Embodiment 3
[0030] (1) Add 25 parts of water-based acrylic resin, 50 parts of pigment, 6 parts of Digo dispersant 760W, 20 parts of water, 15 parts of ethanol and 0.5 part of defoamer into a high-speed mixer for pre-dispersion. The stirring speed is controlled by a frequency conversion motor. Stir slowly to prevent the slurry from spilling, then stir at a high speed of 1000-2000 rpm to make the mixture even;
[0031] (2) Put the pre-dispersed slurry into the sand mill for sanding; the particle size of the sanded slurry is less than 10um.
[0032] (3) Add acrylic emulsion to the slurry after sanding, wherein the amount of acrylic emulsion is 30%, the amount of slurry is 60%, stir and mix evenly, and add solvent at the same time so that the viscosity of the ink is Tu 4 viscosity cup 20 -30s, the solvent is water and ethanol, and the volume ratio of water and ethanol is 2:1. The prepared ink has excellent pigment dispersibility and good stability, and the ink does not thicken or unite after...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com