Method for preparing sheepskin clothing leather with small liquid ratio
A sheepskin, liquid ratio technology, applied in leather impregnation, small raw hide/large raw hide/leather/fur treatment, small raw hide/large raw hide/leather/fur mechanical treatment, etc. Sewage volume, water consumption and other problems, to achieve the effect of feeling plump, soft and elastic, reducing water consumption, and fine leather
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0059] The method for preparing sheepskin garment leather with small liquid ratio comprises the following steps:
[0060] (a) Carry out pretreatment to the sheep skin of soil species in the groove, and the pretreatment includes soaking, washing, re-immersing, shearing, fleshing and degreasing in sequence, wherein the intermittent rowing is 1 minute per hour. frequency;
[0061] Wherein, the immersion is carried out with the first mixed aqueous solution, and the liquid ratio is 10; in terms of volume of water, the first mixed aqueous solution contains 1.5g / L of Eliite wetting agent HAC and 0.3g / L of antiseptic and bactericide; The temperature is 25°C, paddle for 2 minutes after soaking for 2.5 hours, and then paddle intermittently. The total time of soaking in water is 17 hours;
[0062] The skin washing is carried out with the second mixed aqueous solution with a liquid ratio of 10; calculated by the volume of water, the second mixed aqueous solution contains Eliite degreasin...
Embodiment 2
[0076] The method for preparing sheepskin garment leather with small liquid ratio comprises the following steps:
[0077] (a) Carry out pretreatment to the sheep skin of the soil species in the trough. The pretreatment includes immersion, washing, re-immersion, shearing, de-fleshing and degreasing in sequence. The intermittent padding is 2 minutes per hour. frequency;
[0078] Wherein, the immersion is carried out with the first mixed aqueous solution, and the liquid ratio is 9; in terms of the volume of water, the first mixed aqueous solution contains Eliite wetting agent HAC1.6g / L and antiseptic bactericide 0.35g / L; The temperature is 26°C, paddle for 3 minutes after soaking for 2 hours, and then paddle intermittently. The total time of soaking in water is 14 hours;
[0079] The second mixed aqueous solution is used for skin washing, and the liquid ratio is 11; calculated by the volume of water, the second mixed aqueous solution contains 1.5g / L of Eliite degreasing agent H an...
Embodiment 3
[0093] The method for preparing sheepskin garment leather with small liquid ratio comprises the following steps:
[0094] (a) Carry out pretreatment to the sheep skin of soil species in the groove, and the pretreatment includes soaking, washing, re-immersing, shearing, fleshing and degreasing in sequence, wherein the intermittent rowing is 1 minute per hour. frequency;
[0095] Wherein, the immersion is carried out with the first mixed aqueous solution, and the liquid ratio is 11; in terms of volume of water, the first mixed aqueous solution contains 1.4g / L of Eliite wetting agent HAC and 0.25g / L of antiseptic and bactericide; The temperature is 24°C, paddle for 2 minutes after soaking for 3 hours, and then paddle intermittently. The total time of soaking in water is 20 hours;
[0096] The second mixed aqueous solution is used for skin washing, and the liquid ratio is 9; calculated by the volume of water, the second mixed aqueous solution contains 2.5g / L of Eliite degreasing ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com