Mixed oleoresin printing ink
A technology of resin ink and mixed oil, which can be used in ink, household utensils, applications, etc., and can solve the problem of poor drying performance of soybean oleoresin ink
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] Put 17 parts of water, 10 parts of industrial soybean vegetable oil, 10 parts of tung oil, 10 parts of ethanolamine and 0.5 parts of silicone defoamer in a dispersion cylinder, and uniformly disperse for 2 hours at a speed of 500 r / min Then add 0.5 parts of silicone defoamer, filter, put the filtered emulsion back into the dispersion tank, then add 30 parts of water-soluble acrylic resin, 20 parts of water-based acrylic color paste, and 1 part of soybean lecithin Wetting agent and 0.5 parts of silicone antifoaming agent are uniformly dispersed for 4 hours at a speed of 600 r / min, and finally 0.5 parts of silicone defoaming agent is added and filtered to obtain a mixed oleoresin ink.
Embodiment 2
[0029] Put 12 parts of water, 15 parts of industrial soybean vegetable oil, 15 parts of tung oil, 20 parts of ethanolamine and 0.25 parts of silicone defoamer in a dispersion cylinder, and uniformly disperse for 1 hour at a speed of 600 r / min Then add 0.25 parts of silicone defoamer, filter, put the filtered emulsion back into the dispersion tank, then add 25 parts of water-soluble acrylic resin, 10 parts of water-based acrylic color paste, and 2 parts of soybean lecithin Wetting agent and 0.25 parts of silicone antifoaming agent are uniformly dispersed for 2 hours at a speed of 800 r / min, and finally 0.25 parts of silicone defoaming agent is added and filtered to obtain a mixed oleoresin ink.
Embodiment 3
[0031] Put 8 parts of water, 20 parts of industrial soybean vegetable oil, 20 parts of tung oil, 15 parts of ethanolamine and 0.25 parts of silicone defoamer in a dispersion cylinder, and uniformly disperse for 1.5 hours at a speed of 550 r / min Then add 0.25 parts of silicone defoamer, filter, put the filtered emulsion back into the dispersion tank, then add 20 parts of water-soluble acrylic resin, 15 parts of water-based acrylic color paste, and 1 part of soybean lecithin Wetting agent and 0.25 parts of silicone antifoaming agent are uniformly dispersed for 3 hours at a speed of 700 r / min, and finally 0.25 parts of silicone defoaming agent is added and filtered to obtain a mixed oleoresin ink.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com