A glass coating, water-based technology, applied in the field of coatings, can solve the problems of high construction environment requirements, low efficiency, and slow drying of water-based glass paint, and achieve the effects of high construction efficiency, convenient construction, and less volatiles
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] formula:
[0032] Bayer waterborne UV polyurethane dispersion Bayhydrol UV XP 2629 85 parts by weight;
[0033] 1.5 parts by weight of BYK025 defoamer;
[0034] BYK333 leveling agent 0.5 parts by weight;
[0035] 5 parts by weight of deionized water;
[0036] 0.2 parts by weight of triethylamine pH regulator;
[0037] Rohm and Haas RM-2050D 0.3 parts by weight;
[0038] 1.5 parts by weight of 1173 photoinitiator;
[0039] 2 parts by weight of W-T507 adhesion promoter;
[0040] 5 parts by weight of 5378 sand flour.
[0041] making process:
[0042] Add water-based UV polyurethane dispersion, deionized water, PH regulator, thickener and defoamer into the reaction kettle in sequence, and then add the leveling agent and adhesion promoter in sequence after the medium-speed dispersion is uniform, and after 10 minutes of medium-speed dispersion Add photoinitiator and sand flour and disperse at low speed for 3 minutes to obtain the water-based UV glass coating.
[0043...
Embodiment 2
[0045] formula:
[0046] Bayer waterborne UV polyurethane dispersion Bayhydrol UV XP 2629 85 parts by weight;
[0047] 2 parts by weight of BYK025 defoamer;
[0048] BYK333 leveling agent 0.5 parts by weight;
[0049] 3.5 parts by weight of deionized water;
[0050] 0.2 parts by weight of triethylamine pH regulator;
[0051] Rohm and Haas RM-2050D 0.3 parts by weight;
[0052] 1.5 parts by weight of 1173 photoinitiator;
[0053] 2 parts by weight of W-T507 adhesion promoter;
[0054] 5 parts by weight of 5378 sand flour;
[0055] SY7000 matting powder 0.5 parts by weight.
[0056] making process:
[0057] Add water-based UV polyurethane dispersion, deionized water, PH regulator, thickener and defoamer to the reaction kettle in sequence, disperse at medium speed evenly, add matting powder and disperse at medium speed for 10 minutes, disperse to fineness ≤ 30 microns, and then Add leveling agent and adhesion promoter in sequence, disperse at medium speed for 10 minutes, t...