Embodiment 1
[0025] (1) Prepare 100 kg of component A material: Weigh 51 kg of polypropylene oxide ether polyol with 6 functionalities and a molecular weight of 800, 19 kg of polyether polyol GJ-480219 kg, and 0.3 kg of water, and put them into a mixing kettle Stir well; add 0.2 kg of dibutyltin mercaptide, 0.2 kg of lead isooctanoate, 0.4 kg of 2,4,6-tris(dimethylaminomethyl)phenol, 0.4 kg of bismorpholine diethyl ether, phthalic acid 28.5 kilograms of dioctyl esters, stir evenly.
[0026] (2) Prepare 100 kg of component B materials: put 75 kg of weighed polymethylene polyphenyl polyisocyanate and 25 kg of diphenylmethane diisocyanate into a mixing tank and stir evenly.
[0027] Mix A and B component materials according to the mass ratio of A:B=1:1. After foaming, the polyurethane material for tunnel water plugging can be obtained, and the product index is tested.
[0028]
[0029]
Embodiment 2
[0031] (1) Prepare 100 kilograms of component A materials: Weigh 50 kilograms of polyoxypropylene ether polyols with 6 functionalities and a molecular weight of 800, 225 kilograms of polyether polyols GJ-480, and 0.5 kilograms of water, and put them into a mixing kettle Stir well; add 0.2 kg of dibutyltin mercaptide, 0.2 kg of lead isooctanoate, 0.4 kg of 2,4,6-tris(dimethylaminomethyl)phenol, 0.4 kg of bismorpholine diethyl ether, phthalic acid 23.3 kilograms of dioctyl esters, stir evenly.
[0032] (2) Prepare 100 kg of component B materials: put 75 kg of weighed polymethylene polyphenyl polyisocyanate and 25 kg of diphenylmethane diisocyanate into a mixing tank and stir evenly.
[0033] Mix A and B component materials according to the mass ratio of A:B=1:1. After foaming, the polyurethane material for tunnel water plugging can be obtained, and the product index is tested.
[0034]
Embodiment 3
[0036] (1) Prepare 100 kilograms of component A materials: Weigh 43.5 kilograms of polyoxypropylene ether polyols with 6 functionalities and a molecular weight of 800, 225 kilograms of polyether polyols GJ-480, and 0.3 kilograms of water, and put them into a mixing kettle Stir well; add 0.2 kg of dibutyltin mercaptide, 0.2 kg of lead isooctanoate, 0.4 kg of 2,4,6-tris(dimethylaminomethyl)phenol, 0.4 kg of bismorpholine diethyl ether, phthalic acid Dioctyl ester 30 kilograms, stir evenly.
[0037] (2) Prepare 100 kg of component B materials: put 70 kg of weighed polymethylene polyphenyl polyisocyanate and 30 kg of diphenylmethane diisocyanate into a mixing tank and stir evenly.
[0038] Mix A and B component materials according to the mass ratio of A:B=1:1. After foaming, the polyurethane material for tunnel water plugging can be obtained, and the product index is tested.
[0039] .
PUM
Login to View More Abstract
Description
Claims
Application Information