Environment-friendly, flame-retardant and antibacterial laminated wood floor and manufacturing method thereof
A technology for strengthening wooden floors and manufacturing methods, which can be used in manufacturing tools, wood treatment, flat products, etc., can solve the problems of mildew, bacteria breeding, and easy deformation, so as to prevent bacteria from breeding, reduce skin swelling, and restore skin. The effect of vitality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] A method for manufacturing environmentally friendly flame-retardant and antibacterial laminated wood flooring, comprising the following steps:
[0030] S1: Wood or straw is used to produce fibers by traditional methods of producing fiberboards; generally, fibers that can be used to produce high-density boards are obtained after cutting, screening, crushing, washing, mechanical fiber separation, and pulping.
[0031] S2: Drying the fiber, the water content of the fiber after drying is 5% by weight; when drying, the airflow drying method can be used, and other methods can also be used.
[0032] S3: Add 5% of the dry fiber weight mixed glue to the dry fiber, stir evenly and lay it into a slab for pre-pressing;
[0033] Described mixed glue is made up of following composition:
[0034] In parts by weight, 45 parts of isocyanate resin glue, 30 parts of soybean protein glue, 5 parts of sodium dodecyl phenyl ether sulfonate, 5 parts of fir oil, 5 parts of lemon eucalyptus oil...
Embodiment 2
[0045] A method for manufacturing environmentally friendly flame-retardant and antibacterial laminated wood flooring, comprising the following steps:
[0046] S1: Use wood or straw to produce fibers by traditional methods of producing fiberboards; generally, fibers that can be used to produce high-density boards are obtained after cutting, screening, crushing, washing, heating and mechanical fiber separation, and refining.
[0047] S2: Drying the fiber, the water content of the fiber after drying is 6.5% by weight; when drying, the airflow drying method can be used, and other methods can also be used.
[0048] S3: Add mixed glue with 5.2% dry fiber weight to the dry fiber, stir evenly and spread it into a slab for pre-pressing,
[0049] Described mixed glue is made up of following composition:
[0050] In parts by weight, 45 parts of isocyanate resin glue, 30 parts of soybean protein glue, 5 parts of sodium dodecyl phenyl ether sulfonate, 5 parts of fir oil, 5 parts of lemon eu...
Embodiment 3
[0061] A method for manufacturing environmentally friendly flame-retardant and antibacterial laminated wood flooring, comprising the following steps:
[0062] S1: Use wood or straw to produce fibers by traditional methods of producing fiberboards; generally, fibers that can be used to produce high-density boards are obtained after cutting, screening, crushing, washing, heating and mechanical fiber separation, and refining.
[0063] S2: Drying the fiber, the water content of the fiber after drying is 9% by weight; when drying, the airflow drying method can be used, and other methods can also be used.
[0064] S3: Add mixed glue with 5.5% dry fiber weight to the dry fiber, stir evenly and spread it into a slab for pre-pressing,
[0065] Described mixed glue is made up of following composition:
[0066] In parts by weight, 45 parts of isocyanate resin glue, 30 parts of soybean protein glue, 5 parts of sodium dodecyl phenyl ether sulfonate, 5 parts of fir oil, 5 parts of lemon eu...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology