Proportioning method for high-arsenic smoke material for sublimation and arsenic removal
An arsenic dust and arsenic removal technology, which is applied in the direction of improving process efficiency and can solve the problems of low arsenic removal rate and unfavorable high-efficiency production
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0010] Embodiment 1 Rotary kiln (horse boiling furnace method) sublimation dearsenic
[0011] (1) Take 206.18g of reducing high-arsenic dust produced by blast furnace, of which, Pb25%, Sb5%, As 2 o 3 30%, H 2 O3%; (2) Take 153.06g of oxidative high-arsenic fumes produced by the reverberatory furnace, of which, Pb8%, Sb25%, As 2 o 3 40%, H 2 O2%; (3) Mix the above-mentioned two kinds of high-arsenic fumes evenly, and then put the mixed material into an iron pan with a material layer thickness of 10-20mm; (4) Put the iron pan into the horse boiling furnace, heat up to 150°C, and keep it warm for 40 minutes. ⑸The horse boiling furnace continues to heat up to 280°C, and keep it warm for 90 minutes until the smoke is thin; ⑹Continue to heat up in sequence: 320°C, keep warm for 30 minutes; Minutes, the process is over. (8) The weight of the arsenic removal residue is 234.0g, of which, Pb26%, Sb17.8%, As 2 o 3 12.94%, H 2 O0%; ⑼ The weight of dust from arsenic removal is 115...
Embodiment 2
[0014] Example 2 Granulation Shaft Furnace Sublimation Removal of Arsenic
[0015] (1) Take 3075g of reducing dust produced by blast furnace, of which, Pb25%, Sb15%, As 2 o 3 25%, H 2 O2.5%; (2) Take 2218.8g of oxidative dust from lead sintering furnace, of which, Pb16%, Sb28%, As 2 o 3 35%, H 2 O3.2%; (3) mix the above two soot materials evenly in the iron pan; (4) spray and add water in the pan to granulate, and granulate into pellets with a diameter of 1-10mm; (5) sieve 2050g fine particles with a 3mm aperture; ⑹Sieve 2400g spare granules with a sieve with an aperture of 8mm; ⑺Select 2325.5g of granules with a diameter of 3-8mm, containing 14% of granulation water, dry weight 2000g, ingredients: Pb21.24%, Sb20.43%, As 2 o 3 29.17%, placed in a thermal insulation steel pipe with a diameter of 100mm and a leak-proof screen at the bottom, the accumulation ratio of the pellets is 1.65, and the grain consumption height is 179.5mm; 60 minutes; ⑼The temperature of the hot a...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
diameter | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com