A technology of turbine and worm, which is applied in the field of nitriding process of turbine and worm, can solve the problems such as difficult control of nitrogen potential and performance degradation of mechanical parts, etc., and achieve the effect of simple nitriding process, improved performance, and avoiding repetitive procedures

Inactive Publication Date: 2016-06-29
CHONGQING XUXINYUE NC MACHINERY CO LTD
View PDF0 Cites 9 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

In the existing hard nitriding technology, the period is generally 24 to 28 hours, and the nitrided layer reaches 0.2 to 0.3mm. During the nitriding process, the nitrogen potential is not easy to control, and the brittle phase is formed due to the high nitrogen potential, which leads to the performance of mechanical parts. decline

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment Construction

[0009] The technical solution disclosed in the present invention is a nitriding process of a turbine and worm, which is characterized in that it comprises the following steps:

[0010] (1) Clamp the turbine and worm to be nitrided on the special tool, hoist it to the preheating cleaning pool for cleaning, and put it directly into the preheating furnace after cleaning. The temperature of the preheating furnace is 300 ° C, preheating for 2 hours; Heat up the preheating furnace to 480°C and preheat for 2 hours;

[0011] (2) The nitriding process is filled with a mixed gas including ammonia and nitrogen, which is divided into two stages. In the first stage, it is kept at 510-520°C for 10 hours, and the ammonia decomposition rate is 18%-25%; Keep warm at 510-520°C for 10 hours, the ammonia decomposition rate is 30%-50%, and cool down to 200°C with the furnace and air-cooled;

[0012] (3) After the nitriding is completed, hoist it to the cleaning pool after nitriding to cool down, ...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a nitridation process for a worm gear. The nitridation process is characterized by comprising the following steps: (1) clamping a to-be-nitrided worm gear on a special tool, hoisting the to-be-nitrided worm gear to a preheated cleaning pool for cleaning via a crane, then directly putting the cleaned to-be-nitrided worm gear into a preheating furnace with a temperature of 300 DEG C, carrying out preheating for 2 h, then heating the preheating furnace to 480 DEG C and carrying out preheating for 2 h; (2) carrying out nitridation which refers to filling of mixed gas consisting of ammonia gas and nitrogen and comprises two phases, wherein in the first phase, the worm gear is maintained at a temperature of 510 to 520 DEG C for 10 h and an ammonia decomposition rate is 18 to 25%, and in the second phase, the worm gear is maintained at a temperature of 510 to 520 DEG C for 10 h, the ammonia decomposition rate is 30 to 50% and cooling in furnace to 200 DEG C and air cooling out of the furnace are successively carried out; and (3) after completion of nitridation, hoisting the worm gear to a post-nitridation cleaning pool for cooling via the crane, then hoisting the worm gear to a hot-water cleaning pool for cleaning in 8 to 10 min, maintaining the worm gear in the hot-water cleaning pool for 10 min and then hoisting the worm gear in the air so as to allow the worm gear to be rapidly dried. The nitridation process is simple, omits a plurality of repeated procedures, improves work efficiency and enables the overall performance of the worm gear to be greatly improved.

Description

technical field [0001] The invention relates to a turbine worm nitriding process. Background technique [0002] Heat treatment nitriding is nitriding and nitrocarburizing of steel at a temperature of 520°C to 570°C in an atmosphere of ammonia + nitrogen or ammonia + methanol + nitrogen. In recent years, there have been various implementation methods for nitriding and nitrocarburizing processes: for example, pre-vacuuming and filling with ammonia, or ammonia + methanol nitriding treatment process; there is also low vacuum heating first, followed by pulse charging Ammonia gas for nitriding and other processes. In the existing hard nitriding technology, the period is generally 24 to 28 hours, and the nitrided layer reaches 0.2 to 0.3mm. During the nitriding process, the nitrogen potential is not easy to control, and the brittle phase is formed due to the high nitrogen potential, which leads to the performance of mechanical parts. decline. Contents of the invention [0003]...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C23C8/26
Inventor 银琦
Owner CHONGQING XUXINYUE NC MACHINERY CO LTD
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products