Antique finished wood carving manufacturing process

A production process and wood carving technology, which is applied in the field of antique wood carving production process, can solve the problems of poor aesthetic effect, short viewing time, easy cracking of products, etc., and achieve the effect of long service time, beautiful products and good antique effect

Active Publication Date: 2016-08-10
DONGGUAN LIUHUA ART
View PDF6 Cites 4 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] In view of this, the present invention provides an antique woodcarving production process to improve the problems of easy cracking, short viewing time and poor aesthetic effect of products produced by existing processes.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0021] This embodiment provides a kind of antique wood carving production process, comprising the following steps:

[0022] a. Material selection: choose wood that is not easy to corrode, has natural wood grain, and is not easy to deform, cut it, remove debris and dust on the surface of the wood, put the wood in water at 90 ° C, boil for 4 hours, stop the fire, take it out, and air dry it in a cool place until Moisture content is 25%;

[0023] b. One-time drying: put the wood obtained in step a into an oven for baking, the temperature of the oven is controlled at 68°C, bake for 3 hours, and then cool to 20°C;

[0024] c. Sample preparation: engraving the wood obtained in step b to obtain a blank sample;

[0025] d. Burning treatment: use an oxygen lance to carry out burning treatment to the blank sample, the burning time is 2 seconds, and the distance between the oxygen gun and the wood surface is 2 cm, so that the burnt surface area of ​​the wood reaches 75%;

[0026] e. Se...

Embodiment 2

[0033] This embodiment provides a kind of antique wood carving production process, comprising the following steps:

[0034] a. Material selection: choose wood that is not easy to corrode, has natural wood grain, and is not easy to deform, cut it, remove debris and dust on the surface of the wood, put the wood in water at 100 ° C, boil for 6 hours, stop the fire, take it out, and air dry it in a cool place until Moisture content is 35%;

[0035] b. One-time drying: put the wood obtained in step a into an oven for baking, the temperature of the oven is controlled at 84°C, bake for 5 hours, and then cool to 35°C;

[0036] c. Sample preparation: engraving the wood obtained in step b to obtain a blank sample;

[0037] d. Burning treatment: use an oxygen gun to carry out burning treatment to the blank sample, the burning time is 5 seconds, and the distance between the oxygen gun and the surface of the wood is 8cm, so that the burnt surface area of ​​the wood reaches 85%;

[0038] ...

Embodiment 3

[0045] This embodiment provides a kind of antique wood carving production process, comprising the following steps:

[0046] a. Material selection: Choose wood that is not easy to corrode, has natural wood grain, and is not easy to deform. Cut, remove debris and dust on the surface of the wood, put the wood in water at 95°C, boil for 5 hours, stop the fire, take it out, and air dry it in a cool place until Moisture content is 30%;

[0047] b. One-time drying: put the wood obtained in step a into an oven for baking, the temperature of the oven is controlled at 76°C, bake for 4 hours, and then cool to 27°C;

[0048] c. Sample preparation: engraving the wood obtained in step b to obtain a blank sample;

[0049] d. Burning treatment: use an oxygen gun to carry out burning treatment to the blank sample, the burning time is 2.5 seconds, the distance between the oxygen gun and the surface of the wood is 4cm, so that the burnt surface area of ​​the wood reaches 80%;

[0050] e. Secon...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention provides an antique finished wood carving manufacturing process, and relates to the technical field of wood processing. The method comprises several steps of material selection, primary drying, sample manufacturing, fire burning, secondary drying, sanding and repair. A finished product, manufactured by the antique finished wood carving manufacturing process, is not easy to crack, long in preservation time, clear in appearance wood grain and excellent in antiquing effect.

Description

technical field [0001] The invention relates to the technical field of wood processing, in particular to an antique woodcarving production process. Background technique [0002] Antique wood carvings are objects made by imitating the "structure" and "pattern" of ancient objects. Antique woodcarving uses various kinds of wood, such as red sandalwood, black rosewood, rosewood, ebony, red sandalwood and other raw materials to produce various high-end art furniture, screens, pendants, decorations, Buddha statues, art niches, gardens, etc. Antique woodcarving is a fine handicraft created by combining modern technology and traditional handicraft technology, combined with Chinese historical, cultural and artistic elements. Chinese-style classical furniture, wood carvings, various antique furnishings, and replicas of cultural relics are now highly sought after by wealthy Chinese, Chinese and foreigners at home and abroad. [0003] However, the antique wood carvings produced by the...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): B27M1/06B27M1/08B44C1/22B24B29/00B05D7/08
CPCB05D7/08B05D7/584B05D2203/20B05D2451/00B05D2501/00B05D2504/00B24B29/005B27M1/06B27M1/08B44C1/225
Inventor 陈飞
Owner DONGGUAN LIUHUA ART
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products