Zeolite purification fragrance ball and production method thereof
A technology of zeolite and atmosphere ball, applied in the field of air purification, can solve the problems of secondary pollution, consumption of forest resources, destruction of ecological environment, etc., and achieve the effect of preventing electromagnetic radiation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] A method for preparing a zeolite-purified fragrance ball, the weight ratio of the zeolite-purified fragrance ball is as follows:
[0029] 60 parts of zeolite powder;
[0030] 10 parts of diatomaceous earth;
[0031] 5 parts of volcanic rock;
[0032] 5 parts clay;
[0033] Contains the following steps;
[0034] Step 1. Use a ball making machine to initially form zeolite, diatomaceous earth, volcanic rock, and clay into balls in proportion;
[0035] Step 2. Spherical particles of the same size are screened for the first time;
[0036] Step 3, drying;
[0037] Step 4, spray ultrapure water to make ceramic balls;
[0038] Step 5, the second screening selects spherical particles with a diameter of 7 mm;
[0039] Step 6, calcining temperature: 800°C; calcining time: 180 minutes; finally calcined into balls;
[0040] Step 7. After calcination, the damaged ball particles are selected to obtain the final odorless ceramic ball product;
[0041] Step 8. According to the ...
Embodiment 2
[0045] A method for preparing a zeolite-purified fragrance ball, the weight ratio of the zeolite-purified fragrance ball is as follows:
[0046] 80 parts of zeolite powder;
[0047] 20 parts of diatomaceous earth;
[0048] 10 parts of volcanic rock;
[0049] 10 parts clay;
[0050] 5 parts of plant essential oil;
[0051] Contains the following steps;
[0052] Step 1. Use a ball making machine to initially form zeolite, diatomaceous earth, volcanic rock, and clay into balls in proportion;
[0053] Step 2. Spherical particles of the same size are screened for the first time;
[0054] Step 3, drying;
[0055] Step 4, spray ultrapure water to make ceramic balls;
[0056] Step 5, the second screening selects spherical particles with a diameter of 7 mm;
[0057] Step 6, calcining temperature: 1100°C; calcining time: 180 minutes; finally calcined into balls;
[0058] Step 7. After calcination, the damaged ball particles are selected to obtain the final odorless ceramic ball...
Embodiment 3
[0063] A method for preparing a zeolite-purified fragrance ball, the weight ratio of the zeolite-purified fragrance ball is as follows:
[0064] 66 parts of zeolite powder;
[0065] 18 parts of diatomaceous earth;
[0066] 7 parts of volcanic rock;
[0067] 9 parts clay;
[0068] 4 parts of plant essential oil;
[0069] Contains the following steps;
[0070] Step 1. Use a ball making machine to initially form zeolite, diatomaceous earth, volcanic rock, and clay into balls in proportion;
[0071] Step 2. Spherical particles of the same size are screened for the first time;
[0072] Step 3, drying;
[0073] Step 4, spray ultrapure water to make ceramic balls;
[0074] Step 5, the second screening selects spherical particles with a diameter of 7 mm;
[0075] Step 6, calcining temperature: 1000°C; calcining time: 180 minutes; finally calcined into balls;
[0076] Step 7. After calcination, the damaged ball particles are selected to obtain the final odorless ceramic ball p...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology