Embodiment 1
[0031] A method for wood drying treatment, comprising the following steps:
[0032] Step 1. The ambient temperature of the wood drying kiln is heated to 50°C at a heating rate of 2-3°C / h, while the ambient humidity is increased to 90%, and the temperature is kept warm for 2 hours;
[0033] Step 2: Saw the wood into wood blocks or square wood, select the same size and specification and stack them and put them in the preheated wood drying kiln, keep the temperature and humidity in step 1 for 6-8 hours and then release them into the kiln of water vapor;
[0034] Step 3: Adjust the ambient temperature of the wood drying kiln to raise the temperature by program to 80-110°C, which is mainly divided into two stages:
[0035] a. 80-100℃, the heating rate is 8-10℃ / h, and the temperature is kept for 10 hours.
[0036] b. 100-110°C, the heating rate is 11-15°C / h, and the temperature is kept for 24 hours.
[0037] The purpose of these two stages of temperature programming is to promote...
Embodiment 2
[0049] A method for wood drying treatment, comprising the following steps:
[0050] Step 1. The ambient temperature of the wood drying kiln is heated to 55°C at a heating rate of 2-3°C / h, while the ambient humidity is increased to 95%, and the temperature is kept warm for 2 hours;
[0051] Step 2. Saw the wood into wood blocks or square wood, choose the same size and specification and stack them and put them in the preheated wood drying kiln, keep the temperature and humidity in step 1 for 7 hours, and then release the water in the kiln. steam;
[0052] Step 3: Adjust the ambient temperature of the wood drying kiln to raise the temperature by program to 80-110°C, which is mainly divided into two stages:
[0053] a. 80-100°C, the heating rate is 8-10°C / h, and the temperature is kept for 11 hours.
[0054] b. 100-110°C, the heating rate is 11-15°C / h, and the temperature is kept for 26 hours.
[0055] The purpose of these two stages of temperature programming is to promote the...
Embodiment 3
[0067] A method for wood drying treatment, comprising the following steps:
[0068] Step 1. The ambient temperature of the wood drying kiln is heated to 60°C at a heating rate of 2-3°C / h, while the ambient humidity is increased to 100%, and the temperature is kept warm for 3 hours;
[0069] Step 2. Saw the wood into wood blocks or square wood, select the same size and specification and stack them and put them in the preheated wood drying kiln, keep the temperature and humidity in step 1 for 8 hours, and then release the water in the kiln. steam;
[0070] Step 3: Adjust the ambient temperature of the wood drying kiln to raise the temperature by program to 80-110°C, which is mainly divided into two stages:
[0071] a. 80-100°C, the heating rate is 8-10°C / h, and the temperature is kept for 12 hours.
[0072] b. 100-110°C, the heating rate is 11-15°C / h, and the temperature is kept for 28 hours.
[0073] The purpose of these two stages of temperature programming is to promote th...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com