Production method of facial tissue capable of being wetted with water
A production method and paper towel technology are applied in pulp beating/refining methods, papermaking, textiles and papermaking, etc., and can solve problems such as increased raw material cost, production process cost, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0021] A kind of preparation method of wet paper towel adopts the following steps to prepare:
[0022] (1) Put 1610 kg of North American softwood pulp and 1750 kg of Brazilian hardwood pulp into the long and short fiber pulpers respectively, North American softwood pulp, wet weight 18g, knocking degree 12 ° SR, Brazilian hardwood pulp, wet weight 3g, percussion degree 14°SR. Add water to adjust the concentration to 5.5wt% and then disintegrate. The disintegration time is 10 minutes, and then pumped into the long and short fiber pulp pool respectively;
[0023] (2) adjust the concentration of North American softwood pulp to 4.5wt% in the pulp tank before the long fiber tap, enter the refiner, control the energy consumption of refining to 95kwh / t, carry out fiber cutting and splitting, fiber cutting and splitting The wet weight of the mixed wood pulp in the wood pulp after silk broomification is 13g, and the degree of beating is 20°SR, and then enters the long fiber pulp pool a...
Embodiment 2
[0029] A kind of preparation method of wet paper towel adopts the following steps to prepare:
[0030] (1) Put 1,500 kg of North American softwood pulp and 1,500 kg of Brazilian hardwood pulp into the long-fiber pulper and short-fiber pulper respectively. The North American softwood pulp has a wet weight of 20g and a knocking degree of 13°SR, and is made of Brazilian hardwood pulp, wet weight 3g, percussion degree 15 ° SR. Add water to adjust the concentration of the wood pulp to 5.0wt%, then disintegrate for 8 minutes, and then pump it into the long fiber pulp tank and the short fiber pulp tank respectively;
[0031] (2) Add water to adjust the concentration of North American softwood pulp to 4.0wt% in the pulp tank before the long fiber is tapped, and then put it into the first refiner to carry out fiber cutting and fiber separation, after fiber cutting and fiber separation, wood The wet weight of the mixed wood pulp in the pulp is 14g, the beating degree is 22°SR, and then...
Embodiment 3
[0037] A kind of preparation method of wet paper towel adopts the following steps to prepare:
[0038] (1) Put 1,400 kg of North American softwood pulp and 1,600 kg of Brazilian hardwood pulp into the long-fiber pulper and short-fiber pulper respectively. The North American softwood pulp has a wet weight of 21g and a knocking degree of 15°SR, and is made of Brazilian hardwood Pulp, wet weight 4g, percussion degree 16 ° SR. Add water to adjust the concentration of wood pulp to 6.0wt%, then disintegrate for 12 minutes, and then pump them into the long fiber pulp tank and the short fiber pulp tank respectively;
[0039] (2) Add water to adjust the concentration of North American softwood pulp to 4.5wt% in the pulp tank before the long fiber is tapped, and then put it into the first refiner to carry out fiber cutting and fibrillation, after fiber cutting and fibrillation, wood The wet weight of the mixed wood pulp in the pulp is 15g, the beating degree is 24°SR, and then sent to ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com