A high-speed transmission cable for hdmi signal conversion
A high-speed transmission and signal conversion technology, applied in the electronic field, can solve problems such as affecting transmission performance, high labor costs, and difficult to maintain a fixed distance between sub-line centers
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0036] A core wire made of alloy material; the core wire is composed of 1.0% Ni, 0.1% Pt, 0.15% Te, and 98.75% Cu by weight percentage.
[0037] Furthermore, the preparation method of the core wire includes the following steps:
[0038] (1) Take each metal according to the mass ratio, soak it with hydrochloric acid with a mass fraction of 4% for 10 minutes to remove the surface oxide, then clean and dry it with absolute ethanol;
[0039] (2) Heating Cu in a melting furnace to melt it, adding Ni and stirring, until it is completely melted to obtain molten liquid I;
[0040] (3) heating Pt and Te in a melting furnace to melt them to obtain molten liquid II;
[0041] (4) Mix the molten liquid I with the molten liquid II, and stir for 20 minutes to obtain the molten liquid III;
[0042] (5) The molten liquid III is degassed through an online degassing system, and cast at 1100° C. to obtain an ingot with a casting speed of 3 t / h.
[0043] (6) After the ingot is rolled, it is rap...
Embodiment 2
[0046] A core wire made of alloy material; the core wire is composed of Ni1.2%, Pt0.3%, Te0.55%, Cu97.95% by weight percentage.
[0047] Furthermore, the preparation method of the core wire includes the following steps:
[0048] (1) Take each metal according to the mass ratio, soak it with hydrochloric acid with a mass fraction of 4% for 15 minutes to remove surface oxides, then clean and dry it with absolute ethanol;
[0049] (2) Heating Cu in a melting furnace to melt it, adding Ni and stirring, until it is completely melted to obtain molten liquid I;
[0050] (3) heating Pt and Te in a melting furnace to melt them to obtain molten liquid II;
[0051] (4) Mix the molten liquid I with the molten liquid II, and stir for 15 minutes to obtain the molten liquid III;
[0052] (5) The molten liquid III is degassed through an online degassing system, and cast at 1150° C. to obtain an ingot with a casting speed of 3 t / h.
[0053] (6) After the ingot is rolled, it is rapidly cooled t...
Embodiment 3
[0056] A core wire made of alloy material; the core wire is composed of 1.0% Ni, 0.25% Pt, 0.40% Te, and 98.35% Cu by weight percentage.
[0057] Furthermore, the preparation method of the core wire includes the following steps:
[0058] (1) Take each metal according to the mass ratio, soak it with hydrochloric acid with a mass fraction of 4% for 15 minutes to remove surface oxides, then clean and dry it with absolute ethanol;
[0059] (2) Heating Cu in a melting furnace to melt it, adding Ni and stirring, until it is completely melted to obtain molten liquid I;
[0060] (3) heating Pt and Te in a melting furnace to melt them to obtain molten liquid II;
[0061] (4) Mix the molten liquid I with the molten liquid II, and stir for 12 minutes to obtain the molten liquid III;
[0062] (5) The molten liquid III is degassed through an online degassing system, and cast at 1120° C. to obtain an ingot at a casting speed of 3 t / h.
[0063] (6) After the ingot is rolled, it is rapidly...