Steaming dye fixing technology for wool fiber
A wool fiber and steaming technology, which is applied in the field of wool dyeing treatment, can solve the problems that are not conducive to color fixation and green wool production, and achieve the effect of improving level dyeing and penetration dyeing
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] The steam dyeing fixation process of embodiment 1 wool fiber comprises the following steps:
[0018] S1, configure wool fibers, place the wool fibers in high-pressure steam equipment, conduct a steaming treatment at 110°C, then take them out and dry them;
[0019] S2: Dye the steamed wool in a reactive dye mixed solution at 60°C, where the composition of the reactive dye mixed solution includes reactive dye 2% (o.m.f), glacial acetic acid 6% (o.m.f), NT02 type wool low temperature dyeing Auxiliary 2% (o.m.f), wool penetrant 6g / L, sodium sulfide 35g / L, Pingpingjia 0.5g / L, ammonium sulfate 3g / L;
[0020] S3: Soaping, drying, placing the dried wool in high-pressure steam sterilization equipment, and performing a second steaming treatment at 110°C;
[0021] S4: wash again with distilled water, and dry.
[0022] The treatment time of one steaming treatment in S1 is 30min.
[0023] The processing time of the secondary steaming treatment in S3 is 120s.
Embodiment 2
[0025] The difference between embodiment 2 and embodiment 1 is that
[0026] S1 The steaming temperature is 130°C, and the steaming time is 30 minutes;
[0027] S2: Dye the steamed wool in a reactive dye mixed solution at 60°C, where the composition of the reactive dye mixed solution includes reactive dye 2% (o.m.f), glacial acetic acid 6% (o.m.f), NT02 type wool low temperature dyeing Auxiliary 2% (o.m.f), wool penetrant 6g / L, sodium sulfide 35g / L, Pingpingjia 0.5g / L, ammonium sulfate 3g / L;
[0028] S3: The secondary steaming treatment temperature is 110°C, and the treatment time is 60s.
[0029] The wool in S1 is wool pretreated with urea. The urea pretreatment is as follows: immerse the wool in urea aqueous solution at 70-90°C for 5 minutes, and dry at low temperature. The concentration of urea in the urea aqueous solution is 40g / L.
Embodiment 3
[0031] The difference between embodiment 3 and embodiment 2 is that the steaming temperature of S1 is 120° C., and the steaming time is 35 minutes;
[0032] S2: Dye the steamed wool in a reactive dye mixed solution at 55°C, where the composition of the reactive dye mixed solution includes 2.5% (o.m.f) reactive dye, 5% (o.m.f) glacial acetic acid, low-temperature dyeing of NT02 wool Auxiliary 2.5% (o.m.f), wool penetrant 4.5g / L, sodium sulfide 42g / L, Pingpingjia 0.4g / L, ammonium sulfate 5.5g / L;
[0033] S3: The secondary steaming treatment temperature is 100°C, and the treatment time is 90s.
[0034] The wool in S1 is wool pretreated with urea. The urea pretreatment is as follows: soak the wool in urea aqueous solution at 80°C for 3 minutes, and dry at low temperature. The concentration of urea in the urea aqueous solution is 55g / L.
[0035] The urea aqueous solution also contains penetrant JFC.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com