Glass etching solution, preparation method of glass etching solution and method for preparing anti-glare glass with glass etching solution
An etching solution and anti-glare technology, which is applied in the field of vehicle-mounted anti-glare glass preparation, can solve problems such as interfering with the correct judgment of drivers and passengers, vehicle driving and personal safety hazards, and achieve homogenization of grain size and improvement of suspension capacity , The effect of slowing down the etching reaction speed
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A kind of glass etchant, is made up of the raw material of following percentage by weight: citric acid 10%, acetic acid 10%, NH 4 F 25%, (NH 4 ) 2 SiF 6 5%, K 2 SiF 6 2.5%, (NH 4 ) 2 HPO 4 10%, viscosity modifier 1.0% (barium sulfate), surfactant 1.0% (sodium dodecylbenzenesulfonate), and the balance is pure water.
[0023] The method for preparing glass etching solution comprises the following steps:
[0024] At a stirring speed of 100 r / min,
[0025] Add acetic acid to water, mix well, then add citric acid, NH 4 F, (NH 4 ) 2 HPO 4 , after mixing, add (NH 4 ) 2 SiF 6 and K 2 SiF 6 , mix well, add a viscosity modifier and a surfactant, mix well, and age for 4 hours to obtain a glass etching solution.
[0026] The method for preparing anti-glare glass by using glass etching solution comprises the following steps:
[0027] Immerse the glass cleaned with pure water into the glass etching solution, let it stand for 90 seconds, polish it for 25 minutes, s...
Embodiment 2
[0030] A kind of glass etchant, is made up of the raw material of following percentage by weight: citric acid 7.5%, acetic acid 6.5%, NH 4 F 27%, (NH 4 ) 2 SiF 6 7.5%, K 2 SiF 6 1.5%, (NH 4 ) 2 HPO 4 7%, viscosity regulator 1.2% (propylene glycol alginate), surfactant 0.6% (sodium lauryl sulfate), and the balance is pure water.
[0031] The method for preparing glass etching solution comprises the following steps:
[0032] At a stirring speed of 50 r / min,
[0033] Add acetic acid to water, mix well, then add citric acid, NH 4 F, (NH 4 ) 2 HPO 4 , after mixing, add (NH 4 ) 2 SiF 6 and K 2 SiF 6 , mix well, add a viscosity modifier and a surfactant, mix well, and age for 12 hours to obtain a glass etching solution.
[0034] The method for preparing anti-glare glass by using glass etching solution comprises the following steps:
[0035] Immerse the glass cleaned with pure water into the glass etching solution, let it stand for 120 seconds, polish it for 30 m...
Embodiment 3
[0038] A kind of glass etchant, is made up of the raw material of following percentage by weight: citric acid 13%, acetic acid 10%, NH 4 F 21%, (NH 4 ) 2 SiF 6 9%, K2 SiF 6 2%, (NH 4 ) 2 HPO 4 10%, viscosity regulator 0.8% (polyanionic cellulose), surfactant 1.2% (sodium dodecylbenzenesulfonate), and the balance is pure water.
[0039] The method for preparing glass etchant and the method for preparing anti-glare glass with glass etchant refer to Example 1.
[0040] After testing, the anti-glare glass has a gloss of 128, a haze of 8.5%, and a roughness of 0.042 μm. 075μm。 The current car anti-glare glass has a haze of 0.6% and a roughness of 0.075μm.
PUM
Property | Measurement | Unit |
---|---|---|
surface roughness | aaaaa | aaaaa |
haze | aaaaa | aaaaa |
surface roughness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com